# Fileset

[2026_Shimokawa_Nat Commun_Electrode-free bioelectrochemical intercalation for scalable lithium recovery.pdf](https://mdr.nims.go.jp/filesets/a3d0f332-d2f7-462b-b3aa-dcf4ac78bf92/download)

## Creator

Kohei Shimokawa, Duyen Minh Pham, Heng Yi Teah, Xizi Long, Yasunori Kikuchi, [Akihiro Okamoto](https://orcid.org/0000-0002-8102-4316)

## Rights

[Creative Commons BY-NC-ND Attribution-NonCommercial-NoDerivs 4.0 International](https://creativecommons.org/licenses/by-nc-nd/4.0/)

## Other metadata

[Electrode-free bioelectrochemical intercalation for scalable lithium recovery](https://mdr.nims.go.jp/datasets/89954fa8-e767-4854-baa4-ddea5397672e)

## Fulltext

Electrode-free bioelectrochemical intercalation for scalable lithium recovery  Article https://doi.org/10.1038/s41467-026-74500-3 Electrode-free bioelectrochemical intercalation for scalable lithium recovery Kohei Shimokawa 1,2,3,11 , Duyen Minh Pham3,4,11, Heng Yi Teah5, Xizi Long 3, Yasunori Kikuchi 5,6,7 \& Akihiro Okamoto 3,4,8,9,10 Electrochemical intercalation materials offer selective lithium recovery from saline streams, but conventional electrode architectures impose scale-up constraints. Here we report an electrode-free bioelectrochemical intercalation process in which a dissimilatory metal-reducing bacterium, Shewanella onei- densisMR-1, drives lithiumuptake into λ-MnO2. The system self-assembles into microbe–mineral agglomerates that sustain electrochemical-rate intercalation without external wiring, forming a recoverable lithiated slurry. Over 95% of lithium was recovered from seawater within hours, with less than 1% co- intercalation of competingmetal ions. Bottom-up self-agglomeration, inwhich extracellular and cell-surface cytochromes facilitate efficient electron transfer, enables scale-up. The generality and energetic basis of this mechanism are further supported by reproducing the key behaviour in an orthogonal FePO4 host with negligible abiotic reactivity. Techno-economic and life-cycle ana- lyses for Li2CO3 production suggest that the process reduces brine water loss while maintaining competitive costs. These results establish self-assembled bioelectrochemical intercalation as a route to lithium recovery from saline streams. Li, an essential component of rechargeable batteries, is pervasive in nature, yet its distribution exhibits considerable heterogeneity1–8. Historically, the exploitation of high-concentration Li reserves, such as brines and ores, has been the primary focus. However, the escalating global demand for large-scale Li-ion batteries (LIBs) has exposed the constraints of regional availability and the detrimental environmental repercussions associated with conventional evaporative Li recovery from brines and ore refining3,9,10. Consequently, there is a burgeoning need to develop environmentally benign Li recovery methods that demonstrate improved energy efficiency and enable the utilization of diverse Li sources1–3,10,11. Among the various alternative approaches, electrochemical techniques employing electrode materials for LIBs, such as λ-MnO2 and FePO4, demonstrate remarkable ability for rapid and selective Li recovery from sources with a range of concentrations, including low-concentration seawater (Supplementary Table 1)5,11–22. However, inherent limitations associated with two-dimensional elec- trode fabrication, includingmass loading of electroactivematerial and ohmic drop, pose challenges to the scale-up of efficient and sustain- able electrochemical Li recovery systems1,3–6. Dissimilatory metal-reducing bacteria are ubiquitous in low- oxygen marine and freshwater environments23,24. These bacteria cou- ple anaerobic respiration of organic compounds linked to the Received: 27 March 2026 Accepted: 8 June 2026 Check for updates 1Frontier Research Institute for Interdisciplinary Sciences, Tohoku University, Sendai, Japan. 2Institute for Materials Research, Tohoku University, Sendai, Japan. 3International Center forMaterials Nanoarchitectonics (WPI-MANA), National Institute for Materials Science, Tsukuba, Japan. 4ResearchCenter for Macromolecules and Biomaterials, National Institute for Materials Science, Tsukuba, Japan. 5Presidential Endowed Chair for “Platinum Society”, The University of Tokyo, Tokyo, Japan. 6Department of Chemical System Engineering, The University of Tokyo, Tokyo, Japan. 7Institute for Future Initiatives, The University of Tokyo, Tokyo, Japan. 8Graduate School of Chemical Sciences and Engineering, Hokkaido University, Sapporo, Japan. 9Graduate School of Science and Technology, University of Tsukuba, Tsukuba, Japan. 10Research Center for Autonomous Systems Materialogy, Institute of Integrated Research, Institute of Science Tokyo (Science Tokyo), Yokohama, Kanagawa, Japan. 11These authors contributed equally: Kohei Shimokawa, Duyen Minh Pham. e-mail: kohei.shimokawa.b7@tohoku.ac.jp; ykikuchi@ifi.u-tokyo.ac.jp; okamoto.akihiro@nims.go.jp Nature Communications \|         (2026) 17:5400 1 12 34 56 78 9 0 () :,; 12 34 56 78 9 0 () :,;[http://orcid.org/0000-0003-3261-9679](http://orcid.org/0000-0003-3261-9679)[http://orcid.org/0000-0003-3261-9679](http://orcid.org/0000-0003-3261-9679)[http://orcid.org/0000-0003-3261-9679](http://orcid.org/0000-0003-3261-9679)[http://orcid.org/0000-0003-3261-9679](http://orcid.org/0000-0003-3261-9679)[http://orcid.org/0000-0003-3261-9679](http://orcid.org/0000-0003-3261-9679)[http://orcid.org/0000-0002-0502-5675](http://orcid.org/0000-0002-0502-5675)[http://orcid.org/0000-0002-0502-5675](http://orcid.org/0000-0002-0502-5675)[http://orcid.org/0000-0002-0502-5675](http://orcid.org/0000-0002-0502-5675)[http://orcid.org/0000-0002-0502-5675](http://orcid.org/0000-0002-0502-5675)[http://orcid.org/0000-0002-0502-5675](http://orcid.org/0000-0002-0502-5675)[http://orcid.org/0000-0003-0002-8233](http://orcid.org/0000-0003-0002-8233)[http://orcid.org/0000-0003-0002-8233](http://orcid.org/0000-0003-0002-8233)[http://orcid.org/0000-0003-0002-8233](http://orcid.org/0000-0003-0002-8233)[http://orcid.org/0000-0003-0002-8233](http://orcid.org/0000-0003-0002-8233)[http://orcid.org/0000-0003-0002-8233](http://orcid.org/0000-0003-0002-8233)[http://orcid.org/0000-0002-8102-4316](http://orcid.org/0000-0002-8102-4316)[http://orcid.org/0000-0002-8102-4316](http://orcid.org/0000-0002-8102-4316)[http://orcid.org/0000-0002-8102-4316](http://orcid.org/0000-0002-8102-4316)[http://orcid.org/0000-0002-8102-4316](http://orcid.org/0000-0002-8102-4316)[http://orcid.org/0000-0002-8102-4316](http://orcid.org/0000-0002-8102-4316)[http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3\&domain=pdf](http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3&domain=pdf)[http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3\&domain=pdf](http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3&domain=pdf)[http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3\&domain=pdf](http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3&domain=pdf)[http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3\&domain=pdf](http://crossmark.crossref.org/dialog/?doi=10.1038/s41467-026-74500-3&domain=pdf)[mailto:kohei.shimokawa.b7@tohoku.ac.jp](mailto:kohei.shimokawa.b7@tohoku.ac.jp)[mailto:ykikuchi@ifi.u-tokyo.ac.jp](mailto:ykikuchi@ifi.u-tokyo.ac.jp)[mailto:okamoto.akihiro@nims.go.jp](mailto:okamoto.akihiro@nims.go.jp)[www.nature.com/naturecommunications](www.nature.com/naturecommunications)electrochemical reduction of extracellular electron acceptors via extracellular electron transfer (EET)23,25. EET-capable bacteria, such as Shewanella oneidensis MR-1, actively attach to the surface of nano- sized metal oxides and connect them with the extracellular or cell- surface enzymes to increase the mineral reduction rate26–28. Given the remarkable ability of thesemicrobes to reducemetal oxides, EET could be a promising driving force to electrochemically recover Li without using electrodes. To date, EET has primarily been employed for modifying the oxidation state of several transitionmetals (e.g., Cr, Mn, Fe, and Co)29–31, leaving the manipulation of alkali and alkaline-earth metals unexplored. In this study, we examine bioelectrochemical intercalation, wherein dissolved Li ions intercalate into a Li-ion sieve material accompanied by electron donation from microbes (Supplementary Fig. 1). Using this approach, we demonstrate the feasibility of bioe- lectrochemical Li recovery from artificial Li solutions and real sea- water. Furthermore, we evaluate biological mechanisms, cost performance, and environmental impact to assess the scalability of our method. Results MR-1 drives electrode-free Li intercalation Manganese oxides are biocompatible electron acceptors under anae- robic conditions forMR-1 andother EET-capablebacteria27,32,33. λ-MnO2 with a spinel structure was chosen from the reported Li-ion sieve materials considering the high Li selectivity due to the three- dimensional diffusion path (Supplementary Fig. 2); its channels are small enough to prevent the intercalation of other metals that abun- dantly exist in brines and seawater (e.g., Na+, K+, and Ca2+)5,9. Further- more, the lithiation potential of λ-MnO2 is substantially higher compared to other MnO2 polymorphs (Supplementary Fig. 3)34, resulting in a large driving force for Li intercalation. We first examined Li recovery from LiCl solutions dissolved in phosphate-buffered saline (PBS) at pH 7.4 and at high concentrations of Na+ and K+. The synthesized λ-MnO2 nanoparticles, whose lattice constant was determined to be \~8.037 Å (Supplementary Fig. 4), and MR-1 were anaerobically incubated with 50mM LiCl/PBS in the pre- sence of lactate as the electron donor for 24 h at 30 °C. Contrary to the expectation that bacterial EET would promote MnO2 dissolution 27, the λ-MnO2 nanoparticles remained in a solid state and self-organized into sheet-like precipitates (Fig. 1a). Upon mild resuspension, 10–50 µm agglomerates were observed (Fig. 1b), approximately 100 times larger than the initial nanoparticle size (Supplementary Fig. 5). Bacterial cells were intimately associated with the mineral matrix and further inte- grated them into \>100μm structure, as confirmed by fluorescence microscopy of DNA-stained MR-1 (Fig. 1c) and SEM–EDS mapping (Fig. 1d, e). Notably, such large agglomerates did not form in the absence of LiCl (Supplementary Fig. 6), indicating that lithiation trig- gers agglomeration. Structure analyses confirmed that the agglomeration is coupled to Li intercalation. X-raydiffraction (XRD) peaks shifted clearlywithout losing their sharpness (Fig. 2a), indicative of intercalation while maintaining crystallinity. In contrast, such a shift was not observed and the peak intensity decreased when LiCl was omitted from PBS (Sup- plementary Fig. 7), indicating that a Li source is required to prevent reductive dissolution and/or amorphization under these conditions. X-ray absorption near-edge structure (XANES) analysis and inductively coupled plasma optical emission spectroscopy (ICP-OES) indicated Li intercalation to form Li1-xMn2O4 (Fig. 2b and Supplementary Fig. 8). Lactate was indispensable for MR-1metabolism and lithiation; without lactate, neither process proceeded (Fig. 2c). Consistently, lactate- derivedCO2, negligible acetate production, and a slight decrease in pH correlatedwith the electrochemical capacity (Supplementary Fig. 9), in line with a bioelectrochemical reduction pathway. In contrast, abiotic chemical reduction of λ-MnO2 by lactate could partially allow Li intercalation but cause a crystallinity loss (Supplementary Fig. 10). Importantly, acetate and other possible products (i.e., pyruvate, for- mate, acetaldehyde) at observed concentration ranges could not explain the extent of bioelectrochemical Li intercalation (Supple- mentary Figs. 11–13), indicating negligible contributions of diffusible metabolic reductants. Furthermore, abiotic λ-MnO2 reduction ceased within several hours (Supplementary Fig. 14), while biotic reaction Fig. 1 \| Self-agglomeration of Shewanella oneidensis MR-1 and λ-MnO2 nano- particles. a Agglomeration occurring at the bottom of the reactor after bioelec- trochemical Li recovery in 50mM LiCl/PBS solution with 50mM lactate. b Microscopic image of the resuspended precipitate. c Fluorescent microscopy image of an agglomerate with DNA-stained MR-1 cells prepared via DAPI staining. d SEMand (e) EDSmapping images for a small pieceof agglomerate formed in LiCl/ PBS. Similar micrographic results were obtained in at least two independent experiments. Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 2[www.nature.com/naturecommunications](www.nature.com/naturecommunications)continuously proceeded until the end state. Given that the chemical lithiation formed an intermediate LixMn2O4 (x = \~0.5), the less ener- getically favourable reaction (x \> \~0.5) is principally driven by micro- bial electron input. These results demonstrate that microbial metabolism accelerates Li intercalation beyond the chemically acces- sible intermediate states while preserving material integrity, estab- lishing a distinct bioelectrochemical intercalation mechanism hardly achievable by purely chemical processes. The selectivity of Li intercalation was further confirmed using Li–Mgmixed solutions. Although λ-MnO2 prevents the intercalation of other alkali metals, this was not the case for Mg2+ because its ionic radius is similar to that of Li+35. Themolar ratio of Li/Mgwas 200–1000 times more concentrated in the agglomerates compared to the solu- tion (Fig. 2d). This is reasonable from the kinetic analysis, in that the order was consistent with the difference in diffusion distances esti- mated from their activation energies (Supplementary Fig. 15). Such slow kinetics ofMg2+ diffusion in spinel-oxidematerials arewell known in the field of Mg-ion batteries36–38. The intercalation of Na+ and K+ was negligible (Supplementary Table 2), even though they were abundant in PBS solutions. Furthermore, the XRD and XANES profiles of inter- mediate states prepared by limiting the amount of Li in the vials (Supplementary Figs. 16–19) were consistent with reported electro- chemical charge/discharge of LiMn2O4/λ-MnO2 5,39,40, although the Li depletion led to the above-mentioned crystallinity loss. Therefore, under Li-sufficient conditions, the Li intercalation behaviour exhibited by our bioelectrochemical approach closely resembles that observed in electrode-driven systems. Cell–material interface and electron transfer Direct electron transfer at the cell/particle interface, however, can- not fully explain the spatially homogeneous and efficient lithiation observed within the agglomerates, as a limited number of λ-MnO2 particles directly contact MR-1 cells within the agglomerate (Fig. 1d, e). This suggests the formation of a long-distance electronic network in the agglomerate, comprising semiconductive nanoparticles wired by the extracellular or cell-surface cytochromes28. To analyse the cellular and material interface formed during agglomeration, we performed electron energy loss spectroscopy (EELS) mapping with Fig. 2 \| Bioelectrochemical Li intercalation into λ-MnO2. a XRD patterns and (b) XANES spectra of the materials before and after bioelectrochemical Li recovery in LiCl/PBS and those of LiMn2O4 for reference. c Shift of the 311 peak in the XRD profiles under different conditions of MR-1 and lactate. The inset shows the cor- respondingXRDprofiles \[pink: before Li recovery (i.e., λ-MnO2); purple: w/MR-1, w/ lactate; blue: w/o MR-1, w/o lactate; green: w/o MR-1, w/ lactate; red: w/ MR-1, w/o lactate\], where w/ and w/o represent with and without, respectively. dWeight (left) and selectivity (right) of Li/Mg measured through ICP-OES for the agglomerate prepared in LiCl–MgCl2/PBS solutions with different Li/Mg ratios. In c and d, data are presented as mean values ± standard deviation (s.d.), n = 3 independent bio- logical replicates. Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 3[www.nature.com/naturecommunications](www.nature.com/naturecommunications)scanning transmission electron microscopy (STEM). Subsequent to agglomeration, the Li-containing aggregated material was dispersed by ultrasonication to prepare smaller pieces that could be mounted on a TEM grid. The nanoparticles attached to the cells exhibited no obvious changes in morphology (Fig. 3a), and Mn valency evaluated by EELS decreased from +4 (initial state) to typically around +3.5 (after Li intercalation) even if Mn was not directly attached to the cell (Fig. 3b), consistent with electron delivery beyond immediate cell–particle junctions. Mn was not detected inside the cell through EELS (Fig. 3b), STEM–EDS (Supplementary Fig. 20), or cross-sectional TEM (Supplementary Fig. 21), indicating that Mn-based nanoparticles did not originate fromdissolvedMn ions reduced in the cells. Despite hardly detectable dissolved Mn in the supernatant or its bulky deposition, EELS and TEM results revealed the presence of a small amount of Mn2+ in the vicinity of the microbes (Supplementary Fig. 22). Since this impurity phase was undetectable by XRD, it is most consistent with an amorphous or nanocrystalline hydrated Mn phosphate41. Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 4[www.nature.com/naturecommunications](www.nature.com/naturecommunications)Focused ion beam (FIB)milling with cross-sectional SEM–EDSwas employed for the direct observation of the cellular morphology inside the agglomerates. Note that the agglomerate was subjected to 3,3′- diaminobenzidine (DAB)-H2O2 and OsO4 staining in advance for labelling redox-active enzymes, including cytochromes42. We selected a small piecewith a diameter of 10–20 µm (Supplementary Fig. 23) and subjected it to FIB milling to expose a cross-section (Fig. 3c, d). Os signals were localized near microbes but observed with Mn in the EDS mapping (Fig. 3e–g and Supplementary Fig. 24). Carbon incorporated in λ-MnO2 was also detected through EDS; the results suggested the expression of the extracellular and cell-surface cytochromes to phy- sically and electrically support the microbial/material composite. In addition, we observed a nanowire-like structure that facilitates elec- trical conduction via cytochromes23, bridging microbes and nano- particles (Fig. 3h), and suggesting a possible mechanism for electron transfer and agglomerate formation in this system43. EET controls Li intercalation To investigate the critical role of the extracellular and cell-surface cytochromes in agglomeration-coupled Li recovery, we utilized a gene deletion mutant, specifically ΔomcA/mtrC, lacking key outer mem- brane cytochromes (OM c-Cyts), which mediate EET at the solid interface and facilitate long-range electron transfer via membrane vesicles or nanowires23,44. Unlike the wild-type strain, which showed significant λ-MnO2 reduction to the end state (Fig. 3i), theΔomcA/mtrC mutant exhibited incomplete reduction even after 24 h (Fig. 3j), con- firming that full Li intercalation requires cellularmachinery and is not a result of chemical mediation. Fluorescence microscopy of the ΔomcA/ mtrCmutant revealed minimal agglomeration and cellular attachment to the surface of λ-MnO2 (Supplementary Fig. 25), indicating thatOM c- Cyts are key drivers of both EET and the initiation of the microbial–material interactions to agglomerate. Additionally, lever- aging amutant strain45 lacking extracellularpolysaccharide to facilitate OM c-Cyts making contact with λ-MnO2 surface enhanced agglom- erationwith λ-MnO2 and accelerated the rate of Li intercalation relative to the wild type (Supplementary Fig. 26). To further confirm the role of OM c-Cyts in lithiation, we exam- ined the effect of riboflavin, a known non-covalently bound semi- quinone cofactor that enhances direct EET via OM c-Cyts46,47. The addition of 2 µM riboflavin accelerated Li intercalation kinetics by approximately eightfold (Fig. 3k). In contrast, riboflavin alone had a negative effect on abiotic λ-MnO2 reduction by lactate (Supplementary Fig. 27), indicating that the enhancement requires the bacterial EET machinery. Furthermore, rate enhancement by riboflavin was observed in the ΔmtrC mutant but not in the ΔomcA mutant, demon- strating thatboundflavin cofactors specifically accelerate direct EET to λ-MnO2 via OmcA rather than MtrC (Supplementary Fig. 28). Increas- ing the riboflavin concentration up to 100 µM did not enhance the reaction rate (Supplementary Fig. 29), suggesting that indirect electron transport via soluble hydroquinone diffusion plays a negli- gible role under our conditions48. This conclusion was further sup- ported by the absence of enhanced rate in the cell-free supernatant solution obtained from a microbial Li-recovery reactor or from dead cell fractions (Supplementary Fig. 30). These results establish thatMR- 1-driven lithiation proceeds predominantly via a direct EETmechanism involving OM c-Cyts. This directmechanism eliminates the reliance on soluble mediators, whose limited diffusion and concentration often constrain scalability in large-scale processes, thereby reinforcing the practical viability of our bioelectrochemical approach. Scale-up potential of self-assembled agglomerates Time-resolved fractionation experiments further demonstrate that EET does more than supply charge; it nucleates a hierarchically orga- nized solid network that drives process scalability. When the λ-MnO2 nanoparticles and MR-1 cells were incubated under Li-recovery con- ditions, the dry-mass ratio of the suspended (SF) ( \< approximately 10 µm) to the precipitated (PF) fractions declined monotonically while total mass remained constant (Fig. 3l and Supplementary Fig. 31). This shift indicates a transition from dispersed to agglomerated states, rather than mass growth or loss. Concomitantly, Li1-xMn2O4 formed first in SF and later in PF (Fig. 3m, right), demonstrating that Li inter- calation proceeds and then propagates agglomerate growth. Agglomeration was abolished in the control conditions—omitting LiCl or lactate (Supplementary Fig. 32), or deleting the MtrC and OmcA— confirming that EET-driven intercalation is indispensable for these steps (Fig. 3m, l). Consistently, lowering Li concentration suppressed agglomeration (Supplementary Figs. 33–35). Such EET-associated adhesion to solid electron acceptors, together with associated phe- notypic shifts (including the formation of a long-distance electron transfer pathway), is widely observed in microbial–electrode systems under EET conditions28,44. Given that agglomeration concentrates cells and intercalation hosts into a densely packed microenvironment, we envisage that direct EET via the extracellular and cell surface MtrC/ OmcA not only nucleates the self‑agglomerates, but that the resulting architecture can in turn reinforce cellular charge delivery, thereby establishing a biologically mediated positive‑feedback loop that fur- ther accelerates Li intercalation as the agglomerate grows. At the materials level, because smaller particles lithiate faster (Supplementary Fig. 36), EET would initiate at the nanoscale domains, knitting them into 10–50 µmclusterswhoseXRDprofiles converge to a well-crystallized phase irrespective of agglomerate size. This bottom- up self-assembly creates a three-dimensional, electronicallypercolated architecture that retains nanoparticles usually lost in conventional processes49,50, thereby maximizing material utilization. The electro- nically conductive lithiated materials can further accelerate electron flow51,52, establishing a materials-level positive feedback loop that sweeps dispersed particles into the growing network. Such self- assembled living composites circumvent the mass-loading limitations Fig. 3 \| EET-driven electrochemical reaction. a STEM and (b) EELS mapping images for a dispersed composite of MR-1 and nanoparticles after bioelec- trochemical Li recovery. c SEM image after FIBmilling of an agglomerate piece and (d) its enlarged view. e–g EDS mapping images of the cross-section, where Os suggests stained OM c-Cyts. h Enlarged view of the cross-section showing nanowire-like structure (pointed by arrows) along with a cell. Similar micrographic results were obtained in at least two independent experiments. XRD profiles after bioelectrochemical Li recovery from 10mM LiCl/PBS at (i) different reaction times as well as those with (j) a mutant strain lacking OM c-Cyts (ΔomcA/mtrC) and with (k) 2 µM riboflavin (RF) for enhancing the rate of EET. The peak positions of LiMn2O4 and λ-MnO2 are shown by dashed grey lines for comparison. The optical density of theMR-1 cell suspensionwas0.3. lDryweight of the precipitated fraction (PF) and suspended fraction (SF) during the Li recovery process with wild-typeMR- 1, where these fractions were prepared by resuspending the precipitate and then separating the bottom 20% (PF) and the top 80% (SF) after waiting for 1min. Control experiments omitting either MR-1, lactate, or LiCl were carried out, in addition to the case using the mutant strain (ΔomcA/mtrC). Data are presented as mean values ± standard deviation (s.d.), n = 3 independent biological replicates. m Schematics showing the reaction scheme highlighting EET-driven Li intercala- tion, agglomerate formation, and homogeneous Li recovery. The left panel illus- trates the direct EET mechanism from MR-1 to λ-MnO2, where the electrons stemming from lactate are provided to OM c-Cyts while releasing CO2 gas and protons. To further effectively reduce thematerial, bacteria andnanoparticles form agglomerates, likely with bacterial phenotype shift including nanowire formation. As confirmed by control experiments, such as using mutant strains, this agglom- eration is linked to the activity of EET. Thesemicron-scale fractions further grow to form amacroscopic precipitate at the bottom of the reactor during the Li recovery process, as illustrated in the right panel. The illustration was created using Adobe Illustrator. Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 5[www.nature.com/naturecommunications](www.nature.com/naturecommunications)that constrain conventional electrodes4–6, yet deliver comparable Li- recovery rates (Fig. 4a)14,15. By yielding a solid slurry instead of sus- pension, the process minimizes downstream water handling and heat input, providing a mechanistic basis for scalable, energy-efficient Li recovery. Robust Li recovery from real seawater To evaluate the broader applicability of our bioelectrochemical method across a wide range of Li concentrations, we next tested real seawater. Although dissolved Li in seawater (approximately 25μM) is orders of magnitude more abundant than in most freshwater systems11,22, its recovery remains technically demanding2,53,54. We incubated MR-1 cells and λ-MnO2 nanoparticles (5mg) in lactate- supplemented seawater (50mL) under anaerobic conditions. As shown in Fig. 4b, Li was extracted from seawater within several hours, consistent with the PBS-based experiments without riboflavin. In nat- ural seawater, Li removal in the absence of MR-1 was strongly batch dependent; in lactate-supplemented seawater without adding MR-1, Li recovery after 24 h varied from \~20% to \~80% across independent seawater samples (Supplementary Fig. 37). By contrast, inoculation Fig. 4 \| Li recovery from real seawater. a Li recovery performance of this study in seawater (left star) and PBS (right star) comparedwith selected previously reported systems. b Concentration of dissolved Li in real seawater before and after bioe- lectrochemical Li recovery at a seawater/λ-MnO2 ratio of 50mL/5mg. The inset shows the case where only λ-MnO2 was used without MR-1 and lactate. Each plot was from a different sampling batch of seawater. c Bioelectrochemical Li recovery performance after 24 h for 500mL seawater depending on the amount of λ-MnO2. Each plot was coloured by the batch of seawater experiments, and the blue curve is an exponential fit for batch 2, provided as a guide. The blue line indicates the theoretical amount of λ-MnO2 for collecting all Li from 500mL seawater. The inset shows agglomeration formed at the bottom of the reactor with a high seawater/λ- MnO2 ratio of 500mL/1mg. In b and c, the optical density of the MR-1 cell sus- pension was 0.3. d Composition (mass ratio) of Li, Mg, Na, K, and Ca for seawater (left), adsorption (middle), and intercalation (right) into λ-MnO2 during bioelec- trochemical Li recovery. e Schematic diagram showing the reaction mechanisms during bioelectrochemical Li recovery in low-concentration Li sources such as seawater. The potential for Li intercalation shifts due to the Nernst equation by approximately 0.3 V from that in conventional LIBs; however, it is still higher than the typical reduction potential of MR-1 and the dissolution potential of MnO2. Therefore, MR-1 is suitable for obtaining a large driving force for Li intercalation while preventing over-lithiation to form Li2Mn2O4. Furthermore, Li intercalation proceedswithin the electrochemical windowofwater at neutral pH, as indicated by the light blue shadow. The bottom panel summarizes the selective Li intercalation pathwaysduringourbioelectrochemical process. The illustrationwascreatedusing Adobe Illustrator. In b, data are presented as mean values ± standard deviation (s.d.), n = 3 independent biological replicates. Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 6[www.nature.com/naturecommunications](www.nature.com/naturecommunications)with MR-1 cells consistently yielded \~95% recovery under otherwise identical conditions and was accompanied by self-agglomeration, demonstrating that the bioelectrochemical pathway confers robust- ness against matrix-to-matrix variability in the environmental waters. Notably, despite the much lower Li concentration, we did not observe an obvious crystallinity loss under seawater conditions (Supplemen- tary Fig. 38). This contrasts with phosphate-buffered, Li‑depleted conditions, where reductive formation of phosphates occurs once Li becomes limiting. Consistently, λ-MnO2 in seawaterwithout any added reductant (i.e., with neither lactate nor MR-1) removed only \~20% Li presumably via surface adsorption (inset in Fig. 4b). Across thedifferent seawater batches,weobservedmodestbatch- to-batch variations in kinetics, especially before \~3 h (Fig. 4b), con- sistent with the expected compositional variability of environmental samples. Indeed, the Li recovery kinetics were enhanced approxi- mately twofold by spiking 2 μM riboflavin (Supplementary Fig. 39), indicating that the EET-driven intercalation rate can be sensitively modulated by trace redox-active constituents. We further evaluated Li recovery performance at harsh conditions with higher volume and/or higher seawater/λ-MnO2 ratios (Fig. 4c), where the self-agglomeration was observed even at a high ratio of 500mL/1mg (inset in Fig. 4c). The reproducible Li recovery rate against matrix-to-matrix variability was confirmed even for 500mL seawater when the amount of λ-MnO2 was 50mg, while it varied at 5mg or lower. This behaviour is consistent with a capacity-limited regime; the dashed blue line in Fig. 4c indicates the stoichiometric minimum λ-MnO2 required to capture all the Li present in 500mL seawater. Accordingly, the blue curve, an expo- nential fit for batch 2, shows a threshold near this theoretical limit. Even under a challenging condition of 500mL/5mg, the highest utili- zation of the theoretical host capacity reached 42.6%, while main- taining efficient Li recovery from seawater. Remarkably, our method achieved highly selective Li intercalation from seawater (Fig. 4d). This was evaluated by comparing the compositions between the materials soaked in seawater and after bioelectrochemical Li recovery (Supple- mentary Tables 3 and 4). In strong contrast to the non-selectively adsorbed cations, the molar ratios of Li/M (M =Na, Mg, K, Ca) elec- trochemically intercalated into the material were all greater than 100 (Supplementary Table 5). Energetic basis and generality of bioelectrochemical intercalation While the exceptional Li/M selectivity in seawater is ultimately rooted in the intrinsic ion-sieving lattice of λ-MnO2, our advance is to preserve this selectivity at electrochemical rates11, without using any external electrodes. Bacterial EET furnishes the redox potential normally sup- plied by a power source, allowing λ-MnO2 to operate in a fully three- dimensional, self-assembled reactor. In contrast to MnO2-based ion- exchange sorbents22, the continuous bioelectrochemical driving force accelerates ion insertion by an order of magnitude, uniting high dis- crimination with process kinetics previously accessible only to wired electrode systems. Li intercalation into λ-MnO2 to form LiMn2O4 occurs at around 4V vs. Li⁺/Li (approximately 1 V vs. SHE) in con- centrated Li solutions like LIB electrolytes55, whereas the equilibrium potential drops by about 0.3V in seawater due to its low Li con- centration (Fig. 4e). Nevertheless, it is still higher than the potentials of typical MnO2 dissolution 56 and the microbial reduction46, providing a strong driving force for Li intercalation while preventing undesired transformation into over-lithiated Li2Mn2O4 55\. These energetic con- siderations are consistent with the observed microbial–material cou- pling (Fig. 3m). The same concept is further supported by Li intercalation into an FePO4 scaffold (Supplementary Fig. 40), which shows negligible abiotic reactivity under PBS conditions and therefore provides an orthogonal test of the bioelectrochemical driving princi- ple. In addition, alternative electron donors, such as formate, also supported the microbial metabolism coupled to Li intercalation (Supplementary Fig. 41), expanding the choice of electron donors. Together, these results provide a foundation for future optimization strategies, such as pre-treatment of Li sources57 or structural mod- ification of λ-MnO2 17,38, to further enhance Li intercalation efficiency and overall system performance. Techno-economic and life-cycle assessments Finally, we conducted comprehensive techno-economic analysis (TEA) and life-cycle assessment (LCA) to evaluate the prospective process boundary and feasibility of this approach under the assumed config- uration. Considering that electrogenic bacterial strains capable of reducing MnO2 under brine-level salinity conditions have been isolated58, we used data from LiCl/PBS solution experiments to esti- mate the potential for Li2CO3 production from brine sources. In the assumed flow sheet (Supplementary Figs 42 and 43), the process relies on slurry recovery through settling/clarification and dewatering rather than membranes, and the material-clarified brine is subsequently treated in a brine-compatible polishing train before reinjection; these unit operations are included in the TEA/LCA. The following Li recovery process involved oxidizing Li1-xMn2O4 with Na2S2O8 to obtain a Li- containing solution while regenerating λ-MnO2 (Supplementary Fig. 44)57,59, with only a 0.001% Mn loss (Supplementary Fig. 45). Residual bacteria were removed by heating to 90 °C (Supplementary Fig. 46) and further sterilized with Na2S2O8, ensuring that subsequent steps are entirely abiotic. The regenerated λ-MnO2 exhibited low byproduct formation and high structural reversibility (Supplementary Figs. 47 and 48). The Li-containing solution underwent Mn-ion removal, volume reduction, and Li2CO3 precipitation with the addition of Na2CO3, resulting in an industrial-grade purity of ∼98% (Supplementary Fig. 49). Biomass contamination in the delithiated solution was below the detection limit based on biochemical oxygen demand tests. To protect environmental integrity, the spent brine containing bacteria and lactate is treated via a brine-compatiblepolishing train, where they are removed in the aeration tank, clarifier, chlorination, gravity thick- ening and belt pressing, ensuring safe reinjection with minimal water loss (see Supplementary Note 1 for costing assumptions). Under this assumed configuration, the estimated production cost of Li2CO3 using our method is 6.06 USD/kg (Supplementary Fig. 42b), comparable to the commercial direct lithium extraction (DLE) utilizing Li–Al double- layer hydroxides60 aswell as the conventional evaporationmethods for brine sources61–63, and remains below the current market price for similar grade Li2CO3 (Supplementary Table 6). Additionally, our LCA indicated a low water footprint of 0.44 m3eq/kg Li2CO3 (Supplemen- tary Fig. 42c) with minimal brine water loss, significantly out- performing conventional methods60,63, highlighting the potential of our technology to alleviate local water conflicts3,9,10. The estimated climate change impact, 16.99 kg CO2eq/kg Li2CO3 (Supplementary Fig. 42d), was moderately higher than the conventional evaporation methods in Atacama and Olaroz brines63, primarily due to the use of Na2S2O8 (Supplementary Fig. 50). Developing alternative, greener oxidants is therefore a key avenue for further sustainability improve- ments. Crucially, continuous solid/liquid separation for microbial products already sustains approximately 5000 tons per year throughput64,65, underscoring that biotechnological unit operations analogous to our scheme can be scaled seamlessly to the tonnages demanded for commercial brine processing. Our process concentrates Li as a recoverable LixMn2O4 slurry, conferring decisive advantages over both evaporation and adsorption- based DLE routes. Because the product is removed as a solid rather than by bulk-phase boiling, brine water loss isminimal, eliminating the vast evaporative footprint of solar ponds. Unlike sorbent systems, our slurry-based recovery could reduce the need for heated strip solutions, thereby avoiding themajor energypenalty of Li concentration60. The λ- MnO2 host further surpasses the Li–Al double-layer hydroxides in Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 7[www.nature.com/naturecommunications](www.nature.com/naturecommunications)recyclability and intrinsic Li selectivity, while the microbially driven bottom-up self-assembly recovers even nanoscale particles that con- ventional adsorbents discard49,50, minimizing material consumption and raw-material cost. Moreover, cation substitution in the λ-MnO2 framework can further stabilize the lattice while preserving the performance17, offering an additional route to enhance both durability and process economics. In our present TEA/LCA, overall cost and impact are dominated by reagent and heat inputs; reaction rate plays a minor role. Under more kinetically challenging conditions54—for example, ultra-dilute brines—the intrinsically fast, electrochemical-rate Li recovery in our method would widen the performance gap over sorption or evaporation routes, making the advantages reported here a conservative estimate. Discussion In this study, we have demonstrated a scalable bioelectrochemical method for Li recovery, where S. oneidensis MR-1 bacteria autono- mously agglomerate with λ-MnO2 and FePO4, facilitating direct EET and driving Li intercalation with efficacy and selectivity comparable to conventional electrode-based systems. Unlike these methods that are limited by the surface area of electrodes, our bioelectrochemical approach leverages self-organized agglomeration in a homogeneous system, enabling scalability without the need for electrodes with low cost and environmental impact. Although lactate mainly served as the electron donor in this study, this method could also be coupled to microbial metabolic anoxic oxidation of biomass25, offering a low- carbon alternative for large-scale Li recovery4,10. As electron-donating bacteria flourish under various pH and salinity conditions24,58, our approach has broad applicability for diverse Li recovery and recycling scenarios66. Future research should focus on improving the economic and environmental costs associated with oxidants used in Li leaching. For instance, the ability of dissimilatory metal-reducing bacteria to both donate and extract electrons from solids67–69 suggests the pos- sibility of combining microbial Li recovery with biomass-based oxi- dants and microbial electron uptake to further enhance sustainability. Exploring how Li intercalation activates this bacterial phenotype could provide critical insights for future microbial/material interface design. Ultimately, bioelectrochemical intercalation offers a versatile strategy for Li recovery andmay enable broader applications in the handling of alkali and alkaline-earth metals under ambient conditions, as well as advancing materials synthesis, such as electrochemical tuning of intercalation materials for energy and environmental technologies70. Methods Synthesis λ-MnO2 was prepared from LiMn2O4 using an acid-leaching process71. LiMn2O4 particles (0.3 g) were placed in a glass bottle, filled with 0.4M HCl aqueous solution (30mL), and stirred for 24 h at room tempera- ture. The obtainedmaterial was filtered and washed several times with pure water, followed by vacuum drying for 10 h at 100 °C. The syn- thesised λ-MnO2 powder was stored in a desiccator until used in Li recovery experiments. LiMn2O4 was synthesised using a solution combustion method72,73, as briefly described below: LiNO3 (Wako Chemicals, 98%), Mn(NO3)2·6H2O (Wako Chemicals, 98%), and citric acid (Wako Chemicals, 98%) were dissolved in water. The temperature of the solution was carefully increased to evaporate the liquid until a gel was formed. Subsequently, the gelwas ignited by a sudden increase in temperature. Heat treatment was carried out for 4 h at 700 °C in an air atmosphere to increase the crystallinity and decrease the impurity phase. Carbon-coated LiFePO4 (Hohsen Corporation, battery grade) was subjected to K2S2O8 (Sigma-Aldrich, 99%) to prepare FePO4 74\. Typically, 11.7 g of LiFePO4 was stirred at room temperature for 24 h in the solution with 370mL of pure water and 10 g of K2S2O8. The deli- thiatedmaterial was collected by filter paper, washed with pure water, and vacuum-dried for 18 h at 80 °C. All materials were stored in a desiccator before use. VESTA75 was used to visualise the crystal struc- tures of the oxides and the Li diffusion paths. Bacterial preparation Shewanella oneidensis. MR-1 was purchased from ATCC (700550D) and the strain was stored in a deep freezer (−80 °C) before plating on agar plates. The deletion mutant strains were kindly provided by Prof. Kenneth Nealson (University of Southern California) or Prof. Atsushi Kouzuma (Toyo University). The wild-type Shewanella oneidensisMR-1 and the mutant strains lacking OmcA and/or MtrC (ΔomcA/mtrC, ΔomcA, ΔmtrC) and the cell surface polysaccharides (ΔSO3177) were grown aerobically in a Luria-Bertani (LB)medium (10 g/L tryptone, 5 g/ L yeast extract, and 10 g/L NaCl) at 30 °C overnight. Then, the culture was centrifuged for 10min, and the LBmediumwas replaced with PBS (8 g/L NaCl, 0.2 g/L KCl, 0.24 g/L KH2PO4, and 1.44 g/L Na2HPO4; pH 7.4). After removing the LBmedium, the concentration of bacteria was adjusted to the given optical density (OD), typically 0.3, at 600nm before use in Li recovery experiments. Bioelectrochemical Li recovery PBS-based LiCl solutions and real seawater were used for the Li recovery experiments. LiCl (Wako Chemicals, 99%) and lactate (Wako Chemicals, sodium L-lactate solution, 70%) were dissolved in PBS and left overnight to obtain homogeneous solutions. MgCl2 (Wako Che- micals, 97%) was also dissolved to examine the performance in the Li–Mg mixed solutions. Sodium acetate (Wako Chemicals, 98.5%), pyruvate (Nacalai Tesque, 97%), formate (Wako Chemicals, 98%), and acetaldehyde (WakoChemicals, 90%)were used for electron donors in control experiments. Seawater samples were taken from Oarai in Ibaraki, which is on the east side of Japan. Unless otherwise noted, Oarai seawater with 50mM lactate was used for Li recovery experi- ments. The seawater was passed through 0.2 µm sterile filters to remove contaminated cells prior to use. The Li-containing solution and λ-MnO2 nanoparticles were placed in a glass bottle, and dissolved oxygen was eliminated by N2 bubbling. The typical amount of λ-MnO2 used for the experiments with 50mL PBS solution was 50mg. Subsequently, microbes were injected into the reactor, and the mixture was shaken at 30 °C in an incubator. The obtained agglomerates couldbe easily separated from the supernatant liquidbecause theywere attached to the bottomof the reactor, as seen in Fig. 1a. The agglomerates were dispersed in pure water by ultra- sonication and were washed by treatment with 2% Triton X-100 (Sigma-Aldrich) for 15min. The process of centrifugation and repla- cement with pure water was repeated five times to purify the material. Regarding the FePO4 experiment, the washing process was performed in a glove box to suppress the reoxidation of Li-intercalated material. Vacuumdrying at 100 °C for 18 hwas performed to completely remove the water. The Li concentrations before and after Li recovery were analysed through ICP-MS/OES at the Materials Analysis Station, NIMS, and at the Analytical Research Core for Advanced Materials, Institute for Materials Research, Tohoku University. CO2 gas generated from lactate metabolism was measured by a gas chromatography-mass spectrometry (Agilent 7000D) coupled with a HP-PLOT/Q column (30m length, 0.32mm diameter, and 20 µm film thickness). For the time-course experiments, the precipitate was resuspended and stood for 1min, and then the 80% from the top and the remaining 20% were assigned to the suspended and precipitated fractions, respectively. Characterisation XRDwith Cu-Kαwas performed using an X-ray diffractometer (Rigaku, SmartLab) at the NIMS Battery Research Platform. Rietveld analysis was carried out using the RIETAN-FP programme76 to evaluate the lattice constant. The particle size of the synthesised material was evaluated using a nanoparticle tracking analyser (Particle Metrix, ZetaView), where the sample was prepared by ultrasonication to Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 8[www.nature.com/naturecommunications](www.nature.com/naturecommunications)disperse λ-MnO2 nanoparticles in pure water. SEM–EDS (JEOL, JSM- 7800F) of the agglomerate of bacteria and nanoparticles was per- formed at the NIMS Battery Research Platform after a dehydration process. Briefly, the material was immersed in 10% glutaraldehyde overnight, and the supernatant liquid was gradually changed to higher concentrations of ethanol. 100% ethanol was then replaced with tert- butyl alcohol, and thematerial was freeze-dried overnight, followed by Pt coating to increase conductivity. Bright-field and fluorescence images were obtained using an inverted microscope (Leica DMi8, Leica) combined with a micro- camera (Leica, Leica DFC9000). An agglomerate in the culture vial, after decanting to remove the supernatant, was resuspended by pipetting with 5mL of pure water, where the pure water (18.2 MΩ cm) used for this workwas purifiedwith a Direct-Q 5UV system (Millipore). To obtain fluorescence microscopy images of DNA-stained MR-1 cells, 2μL of the resuspended agglomerate was mixed with 2μL of 4′,6- diamidino-2-phenylindole (DAPI, 0.5μg/mL) on a microscope slide, and it was kept in the dark at 4 °C for 3min beforemicroscopy. A DAPI filter was used to obtain fluorescence microscopy images. XANES spectra were obtained at BL-12C, Photon Factory, Japan, where boron nitride (MitsuwaChemicals, 99.5%) was used to dilute the materials for XANES analysis. STEM–EELS (JEOL, JEM-ARM200F) for a microbial/material composite was conducted at the NIMS Battery Research Platform. The original sample was the same as that used for SEM–EDS, but it wasdispersed inethanol to be loadedonto aTEMgrid. The EELS mapping showing the valence state of Mn was obtained by fitting the profile at each point with those of MnO (Mn2+) and MnO2 (Mn4+) as the reference materials. Cross-sections of the agglomerates were characterised by FIB–SEM–EDS (Hitachi, SMF2000), where they were subjected to DAB-H2O2 and OsO4 staining before the analysis. Cross-sectional TEM (JEOL, JEM-1400Plus) was performed using Tokai Electron Microscopy (Nagoya, Japan) for a resin-embedded sample sectioned with an ultramicrotome (Leica, Ultracut UCT). Concentrations of metabolites were analysed by using an ion chromatography system (Shimadzu) equipped with an autosampler (SIL-10Ai), a liquid chromatograph pump (LC-20AD), a degassing unit (DGU-20A 3R), a column oven (CTO-20AC), a conductivity detector (CDD-10A VP), and a communication bus module (CBM-20A). The samples were diluted 100-fold by pure water, and the separation was performed on a non-suppressor column (Shim-pack IC-A3). Standard lines were obtained using a series of organic acid standards, which were prepared in pure water with and without MnCl2 (Wako Che- micals, 99%). The injection volume for all samples and standards was 10 µL. Techno-economic and life-cycle analyses The environmental performanceof our bioelectrochemical Li recovery method was evaluated based on the cradle-to-gate LCA of battery- grade Li2CO3 77 for ease of comparison with current manufacturing63,78. LCAwasperformed in openLCAv2.0with the ecoinvent v3.10database and the ReCiPe 2016 impact assessment method. An extended Li2CO3 precipitation was included based on our experiments described in the main text and Supporting Information. The Li extraction site was modelled on Salar de Atacama63. Within the system, λ-MnO2 and water used for washing and Li concentration were assumed to be recyclable. The life cycle inventory was detailed in Supplementary Tables 7–15. We modelled water consumption and climate change impact to represent the environmental performance of the technology. The background inventory, e.g., environmental loads of general chemical production and electricity generation, was adopted from ecoinvent 3.10, a commercial LCA database. The water consumption was cate- gorized into in-situ water, brine water, and ex-situ water, to distinguish water stress with geography consideration. The climate change impact was characterized by the greenhouse gases’ global warming potential over 100 years79; the contribution was breakdown into Li intercalation or concentration and Li2CO3 precipitation, to differentiate the con- tribution of this study. TEA was conducted based on the same modelled system as the LCA, which assumed a factory producing 70,000-ton Li2CO3 per year andoperating throughout the year (Supplementary Table 16). The cost of Li2CO3 production was calculated based on the annual opera- tion expenditures, including raw materials, utilities, operation and maintenance, overhead, tax and insurance, general expenses, and asset depreciation. The prices of raw materials were obtained from onlinewholesalemarkets inChina and the utility costwas based on the Chilean electricity rate, where the references are listed in Supple- mentary Table 17. We estimated the remaining operation and main- tenace cost and the capital expenditures, represented as asset depreciation, based on an up-flow anaerobic sludge blanket (UASB) facility80. The UASB facility was assumed to resemble the Li intercala- tion facility designed in this study. Statistics and reproducibility For the LCA/TEA: no statistical method was used to predetermine sample size; no data were excluded; randomization and blinding are not applicable to this computational assessment. For bioelec- trochemical observations, similar results were obtained in at least two independent experiments. Reporting summary Further information on research design is available in the Nature Portfolio Reporting Summary linked to this article. Data availability Data that support the findings of this study are available within the paper and the Supplementary Figs. and Tables. Background inventory data for LCA are from the ecoinvent v3.10 database and cannot be redistributed under the ecoinvent licence; these datasets are available to licensed users from ecoinvent (https://ecoinvent.org). The numer- ical data underlying the figures are provided as a Source Data file. Source data are provided with this paper. References 1. Harper, G. et al. Recycling lithium-ion batteries from electric vehi- cles. Nature 575, 75–86 (2019). 2. Swain, B. Recovery and recycling of lithium: a review. Sep. Purif. Technol. 172, 388–403 (2017). 3. Vera, M. L., Torres, W. R., Galli, C. I., Chagnes, A. \& Flexer, V. Environmental impact of direct lithium extraction from brines. Nat. Rev. Earth Environ. 4, 149–165 (2023). 4\. Calvo, E. J. Direct lithium recovery from aqueous electrolytes with electrochemical ion pumping and lithium intercalation. ACS Omega 6, 35213–35220 (2021). 5\. Kim, S., Kang, J. S., Joo, H., Sung, Y.-E. \& Yoon, J. Understanding the behaviors of λ-MnO2 in electrochemical lithium recovery: Key lim- iting factors and a route to the enhanced performance. Environ. Sci. Technol. 54, 9044–9051 (2020). 6\. Romero, V. C. E., Putrino, D. S., Tagliazucchi, M., Flexer, V. \& Calvo, E. J. Electrochemical flow reactor for selective extraction of lithium chloride from natural brines. J. Electrochem. Soc. 167, 120522 (2020). 7\. Tarascon, J.-M. \& Armand, M. Issues and challenges facing rechargeable lithium batteries. Nature 414, 359–367 (2001). 8\. Goodenough, J. B. \& Park, K.-S. The Li-ion rechargeable battery: A perspective. J. Am. Chem. Soc. 135, 1167–1176 (2013). 9\. Battistel, A., Palagonia, M. S., Brogioli, D., La Mantia, F. \& Trocoli, R. Electrochemical methods for lithium recovery: a comprehensive and critical review. Adv. Mater. 32, 1905440 (2020). 10\. Grosjean, C., Miranda, P. H., Perrin, M. \& Poggi, P. Assessment of world lithium resources and consequences of their geographic Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 9[https://ecoinvent.org](https://ecoinvent.org)[www.nature.com/naturecommunications](www.nature.com/naturecommunications)distribution on the expected development of the electric vehicle industry. Renew. Sustain. Energy Rev. 16, 1735–1744 (2012). 11\. Liu, C. et al. Lithium extraction from seawater through pulsed electrochemical intercalation. Joule 4, 1459–1469 (2020). 12\. Trocoli, R., Erinmwingbovo, C. \& La Mantia, F. Optimized lithium recovery from brines by using an electrochemical ion-pumping process based on λ-MnO2 and nickel hexacyanoferrate. Chem- ElectroChem 4, 143–149 (2017). 13\. Lee, J., Yu, S.-H., Kim, C., Sung, Y.-E. \& Yoon, J. Highly selective lithium recovery from brine using a λ-MnO2–Ag battery. Phys. Chem. Chem. Phys. 15, 7690–7695 (2013). 14\. Xu, X. et al. A self-supported λ-MnO2 film electrode used for elec- trochemical lithium recovery from brines. ChemPlusChem 83, 521–528 (2018). 15\. Wang, L. et al. Electrochemical lithium recovery with lithium iron phosphate:What causesperformancedegradation andhowcanwe improve the stability? Sustain. Energy Fuels 5, 3124–3133 (2021). 16\. Lawagon, C. P. et al. Li1−xNi0.33Co1/3Mn1/3O2/Ag for electrochemical lithium recovery from brine. Chem. Eng. J. 348, 1000–1011 (2018). 17\. Lawagon, C. P. et al. Li1−xNi0.5Mn1.5O4/Ag for electrochemical lithium recovery from brine and its optimized performance via response surface methodology. Sep. Purif. Technol. 212, 416–426 (2019). 18\. Hong, H.-J. et al. Highly porous and surface-expanded spinel hydrogen manganese oxide (HMO)/Al2O3 composite for effective lithium (Li) recovery from seawater. Chem. Eng. J. 337, 455–461 (2018). 19\. Chitrakar, R., Makita, Y., Ooi, K. \& Sonoda, A. Lithium recovery from salt lake brine by H2TiO3. Dalton Trans. 43, 8933–8939 (2014). 20\. Chitrakar, R., Kanoh, H., Miyai, Y. \& Ooi, K. Recovery of lithium from seawater using manganese oxide adsorbent (H1.6Mn1.6O4) derived from Li1.6Mn1.6O4. Ind. Eng. Chem. Res. 40, 2054–2058 (2001). 21\. Chitrakar, R., Makita, Y., Ooi, K. \& Sonoda, A. Selective uptake of lithium ion frombrine byH1.33Mn1.67O4 andH1.6Mn1.6O4.Chem. Lett. 41, 1647–1649 (2012). 22\. Li, Z. et al. Continuous electrical pumping membrane process for seawater lithium mining. Energy Environ. Sci. 14, 3152–3159 (2021). 23\. Shi, L. et al. Extracellular electron transfer mechanisms between microorganisms and minerals. Nat. Rev. Microbiol. 14, 651–662 (2016). 24\. Garber, A. I. et al. FeGenie: a comprehensive tool for the identifi- cation of iron genes and iron gene neighborhoods in genome and metagenome assemblies. Front. Microbiol. 11, 37 (2020). 25\. Moradian, J. M., Fang, Z. \& Yong, Y. ‑C.: Recent advances on biomass-fueled microbial fuel cell. Bioresour. Bioprocess. 8, 14 (2021). 26\. Deng, X., Luo, D. \& Okamoto, A. Defined and unknown roles of conductive nanoparticles for the enhancement ofmicrobial current generation: a review. Bioresour. Technol. 350, 126844 (2022). 27\. Myers, C. R. \& Nealson, K. H. Bacterial manganese reduction and growth with manganese oxide as the sole electron acceptor. Sci- ence 240, 1319–1321 (1988). 28\. Nakamura, R., Kai, F., Okamoto, A., Newton, G. J. \& Hashimoto, K. Self-constructed electrically conductive bacterial networks. Angew. Chem. 121, 516–519 (2009). 29\. Lloyd, J. R. Microbial reduction of metals and radionuclides. FEMS Microbiol. Rev. 27, 411–425 (2003). 30\. Belchik, S. M. et al. Extracellular reduction of hexavalent chromium by cytochromes MtrC and OmcA of Shewanella oneidensis MR-1. Appl. Environ. Microbiol. 77, 4035–4041 (2011). 31\. Springthorpe, S. K., Dundas, C. M. \& Keitz, B. K. Microbial reduction of metal-organic frameworks enables synergistic chromium removal. Nat. Commun. 10, 1–11 (2019). 32\. Lovley, D. R. \& Phillips, E. J. Novel mode of microbial energy metabolism: organic carbon oxidation coupled to dissimilatory reduction of iron or manganese. Appl. Environ. Microbiol. 54, 1472–1480 (1988). 33\. Leu, A. O. et al. Anaerobic methane oxidation coupled to manga- nese reduction by members of theMethanoperedenaceae. ISME J. 14, 1030–1041 (2020). 34\. Kitchaev, D. A., Dacek, S. T., Sun, W. \& Ceder, G. Thermodynamics of phase selection in MnO2 framework structures through alkali intercalation and hydration. J. Am. Chem. Soc. 139, 2672–2681 (2017). 35\. Shannon, R. D. Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Crys- tallogr. Sect. A Cryst. Phys. Diffr. Theor. Gen. Crystallogr. 32, 751–767 (1976). 36\. Okamoto, S. et al. Intercalation and push-out process with spinel- to-rocksalt transition on Mg insertion into spinel oxides in magne- sium batteries. Adv. Sci. 2, 1500072 (2015). 37\. Kim, C. et al. Direct observation of reversible magnesium ion intercalation into a spinel oxide host. Adv. Mater. 27, 3377–3384 (2015). 38\. Shimokawa, K. et al. Structure design of long-life spinel-oxide cathode materials for magnesium rechargeable batteries. Adv. Mater. 33, 2007539 (2021). 39\. Kanamura, K., Naito, H., Yao, T. \& Takehara, Z. Structural change of the LiMn2O4 spinel structure induced by extraction of lithium. J. Mater. Chem. 6, 33–36 (1996). 40\. Shiraishi, Y., Nakai, I., Tsubata, T., Himeda, T. \& Nishikawa, F. In situ transmission X-ray absorption fine structure analysis of the charge–discharge process in LiMn2O4, a rechargeable lithium bat- tery material. J. Solid State Chem. 133, 587–590 (1997). 41\. Jin, K. et al. Hydratedmanganese(II) phosphate (Mn3(PO4)2·3H2O) as awater oxidation catalyst. J. Am. Chem. Soc. 136, 7435–7443 (2014). 42\. Deng, X., Dohmae, N., Nealson, K. H., Hashimoto, K. \& Okamoto, A. Multi-heme cytochromes provide a pathway for survival in energy- limited environments. Sci. Adv. 4, eaao5682 (2018). 43\. Nakamura, R., Kai, F., Okamoto, A. \& Hashimoto, K. Mechanisms of long-distance extracellular electron transfer of metal-reducing bacteria mediated by nanocolloidal semiconductive iron oxides. J. Mater. Chem. A 1, 5148–5157 (2013). 44\. Pirbadian, S. et al. Shewanella oneidensisMR-1 nanowires are outer membrane and periplasmic extensions of the extracellular electron transport components. Proc. Natl. Acad. Sci. 111, 12883–12888 (2014). 45\. Kouzuma, A., Meng, X.-Y., Kimura, N., Hashimoto, K. \&Watanabe, K. Disruption of the putative cell surface polysaccharide biosynthesis gene SO3177 in Shewanella oneidensisMR-1 enhances adhesion to electrodes and current generation in microbial fuel cells. Appl. Environ. Microbiol. 76, 4151–4157 (2010). 46\. Okamoto, A., Hashimoto, K., Nealson, K. H. \& Nakamura, R. Rate enhancement of bacterial extracellular electron transport involves bound flavin semiquinones. Proc. Natl. Acad. Sci. 110, 7856–7861 (2013). 47\. Xu, S., Jangir, Y. \& El-Naggar, Y. M. Disentangling the roles of free and cytochrome-bound flavins in extracellular electron transport from Shewanella oneidensis MR-1. Electrochim. Acta 198, 49–55 (2016). 48\. Marsili, E. et al. Shewanella secretes flavins that mediate extra- cellular electron transfer. Proc. Natl. Acad. Sci. 105, 3968–3973 (2008). 49\. Su, J. et al. Continuous flow extraction of lithium from brine using silica-coated LMO beads. Mater. Adv. 6, 2202–2210 (2025). 50\. Disu, B. et al. Review of recent advances in lithium extraction from subsurface brines. Geoenergy Sci. Eng. 241, 213189 (2024). 51\. Kalantarian, M. M., Asgari, S. \& Mustarelli, P. A theoretical approach to evaluate the rate capability of Li-ion battery cathodematerials. J. Mater. Chem. A 2, 107–115 (2014). Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 10[www.nature.com/naturecommunications](www.nature.com/naturecommunications)52\. Li, J. et al. First-principles study of the effect of Ni-doped on the spinel-type Mn-based cathode discharge. ACS Appl. Mater. Inter- faces 15, 8208–8216 (2023). 53\. Chen, X. et al. Spatially separated crystallization for selective lithium extraction from saline water. Nat. Water 1, 808–817 (2023). 54\. Yang, S.,Wang, Y., Pan, H., He, P. \& Zhou, H. Lithiumextraction from low-quality brines. Nature 636, 309–321 (2024). 55\. Thackeray, M. M. Manganese oxides for lithium batteries. Prog. Solid State Chem. 25, 1–71 (1997). 56\. Sun, W., Kitchaev, D. A., Kramer, D. \& Ceder, G. Non-equilibrium crystallization pathways of manganese oxides in aqueous solution. Nat. Commun. 10, 573 (2019). 57\. Pérez-Rodríguez, S., Fitch, S. D., Bartlett, P. N. \& Garcia-Araez, N. LiFePO4 battery material for the production of lithium from brines: effect of brine composition andbenefits of dilution.ChemSusChem 15, e202102182 (2022). 58\. Yadav, S. et al. Geoalkalibacter halelectricus SAP-1 sp. nov. pos- sessing extracellular electron transfer and mineral-reducing cap- abilities from a haloalkaline environment. Environ. Microbiol. 24, 5066–5081 (2022). 59\. Ooi, K., Miyai, Y., Katoh, S., Maeda, H. \& Abe, M. Lithium-ion inser- tion/extraction reaction with λ-MnO2 in the aqueous phase. Chem. Lett. 17, 989 (1988). 60\. Nikfar, S., Fahimi, A. \& Vahidi, E. Unlocking sustainable lithium: a comparative life cycle assessment of innovative extraction methods from brine. Resour. Conserv. Recycl. 212, 107977 (2025). 61\. WSP Ambiental S.A. Technical report summary, operation report, Salar de Atacama. WSP-SQM0011-TRS-Salar-Rev1 (Sociedad Quí- mica y Minera de Chile S. A., 2022). 62\. Huang, T.-Y., Pérez-Cardona, J. R., Zhao, F., Sutherland, J. W. \& Paranthaman, M. P. Life cycle assessment and techno-economic assessment of lithium recovery from geothermal brine. ACS Sus- tain. Chem. Eng. 9, 6551–6560 (2021). 63\. Schenker, V., Oberschelp, C. \& Pfister, S. Regionalized life cycle assessment of present and future lithium production for Li-ion batteries. Resour. Conserv. Recycl. 187, 106611 (2022). 64\. Amasawa, E., Yamanishi, T., Nakatani, J., Hirao,M. \& Sato, S. Climate change implications of bio-based and marine-biodegradable plas- tic: evidence from poly(3-hydroxybutyrate-co-3-hydro- xyhexanoate). Environ. Sci. Technol. 55, 3380–3388 (2021). 65\. Queiroz, S. S., Jofre, F. M., Mussatto, S. I. \& Felipe, M. G. A. Scaling up xylitol bioproduction: challenges to achieve a profitable bio- process. Renew. Sustain. Energy Rev. 154, 111789 (2022). 66\. DuChanois, R. M. et al. Prospects of metal recovery from waste- water and brine. Nat. Water 1, 37–46 (2023). 67\. Ross, D. E., Flynn, J. M., Baron, D. B., Gralnick, J. A. \& Bond, D. R. Towardselectrosynthesis inShewanella: energetics of reversing the Mtr pathway for reductive metabolism. PLoS ONE 6, e16649 (2011). 68\. Okamoto, A., Hashimoto, K. \& Nealson, K. H. Flavin redox bifurca- tion as a mechanism for controlling the direction of electron flow during extracellular electron transfer. Angew. Chem. Int. Ed. 53, 10988–10991 (2014). 69\. Rowe, A. R. et al. Tracking electron uptake from a cathode into Shewanella cells: Implications for energy acquisition from solid- substrate electron donors. mBio 9, e02203-17 (2018). 70\. Lu, Z., Jiang, K., Chen, G., Wang, H. \& Cui, Y. Lithium electro- chemical tuning for electrocatalysis. Adv. Mater. 30, 1800978 (2018). 71\. Hunter, J. C. Preparation of a new crystal form of manganese dioxide: λ-MnO2. J. Solid State Chem. 39, 142–147 (1981). 72\. Varma, A., Mukasyan, A. S., Rogachev, A. S. \& Manukyan, K. V. Solution combustion synthesis of nanoscale materials. Chem. Rev. 116, 14493–14586 (2016). 73\. Shimokawa, K., Matsubara, S., Okamoto, A. \& Ichitsubo, T. Light- induced Li extraction from LiMn2O4/TiO2 in a water-in-salt electro- lyte for photo-rechargeable batteries. Chem. Commun. 58, 9634–9637 (2022). 74\. Ramana, C. V., Mauger, A., Gendron, F., Julien, C. M. \& Zaghib, K. Study of the Li-insertion/extraction process in LiFePO4/FePO4. J. Power Sources 187, 555–564 (2009). 75\. Momma, K. \& Izumi, F. VESTA 3 for three-dimensional visualization of crystal, volumetric andmorphologydata. J. Appl. Crystallogr.44, 1272–1276 (2011). 76\. Izumi, F. \& Momma, K. Three-dimensional visualization in powder diffraction. Solid State Phenom. 130, 15–20 (2007). 77\. Peters, J. F. Best practices for life cycle assessment of batteries.Nat. Commun. 6, 614–616 (2023). 78\. Kelly, J. C., Wang, M., Dai, Q. \&Winjobi, O. Energy, greenhouse gas, and water life cycle analysis of lithium carbonate and lithium hydroxidemonohydrate frombrine and ore resources and their use in lithium ion battery cathodes and lithium ion batteries. Resour. Conserv. Recycl. 174, 105762 (2021). 79\. Huijbregts,M. A. J. et al. ReCiPe, R. I. V.M.: In a harmonized life cycle impact assessmentmethod atmidpoint and endpoint level report I: characterization. National Institute for Public Health and the Envir- onment: Bilthoven, The Netherlands. 1–194 (2016). 80\. Tian, X., Richardson, R. E., Tester, J. W., Lozano, J. L. \& You, F. Ret- rofittingmunicipalwastewater treatment facilities towarda greener and circular economy by virtue of resource recovery: Techno- economic analysis and life cycle assessment. ACS Sustain. Chem. Eng. 8, 13823–13837 (National Institute for Public Health and the Environment, 2020). Acknowledgements The authors thank Dr. Takashi Fujikawa, Dr. Fuyuki Sakamoto, and Dr. Akio Iwanade for their technical help with the materials synthesis and ICP-MS/OES analysis. We also thank Prof. Tetsu Ichitsubo (Tohoku Uni- versity) and Prof.Michael De Volder (University of Cambridge) for fruitful discussions. This research was supported by NIMS Joint Research Hub Program (QN3510) and by JSPS KAKENHI (Grant Number: 22H02265 (A.O.), 20K22460 (K.S.)) and JST, PRESTO (Grant Number: JPMJPR19H1 (A.O.)), Japan. XRD, SEM–EDS, FIB–SEM–EDS, and STEM–EELS analyses were carried out at the NIMS Battery Research Platform. ICP-MS/OES analysis was performed at Materials Analysis Station, NIMS, and at Analytical Research Core for Advanced Materials, Institute for Materials Research, Tohoku University. A part of this work was supported by Advanced Research Infrastructure for Materials and Nanotechnology in Japan (ARIM) of the Ministry of Education, Culture, Sports, Science and Technology (MEXT) (Grant Number: JPMXP1224NM5295). Author contributions K.S., D.M.P., and A.O. conceived and designed this study. A.O. super- vised the project. K.S. and D.M.P. conducted materials synthesis and characterization. K.S., D.M.P., and X.L. carried out Li recovery from PBS and seawater. D.M.P., H.Y.T., and Y.K. performed TEA/LCA. K.S., D.M.P., and A.O. wrote the first draft, and all authors participated in the manu- script revision. Competing interests Research funding related to pilot-scale Li-recovery trials was received from two industrial partners; these partners were not involved in the present study. The authors also hold non-financial collaborations on large-scale MnO2 production and brine testing; no materials from these collaborations were used in this study. K.S., D.M.P., and A.O. filed a patent application for the bioelectrochemical Li recovery method to the Japanese patent office (patent number 7755348). All other authors declare no competing interests. Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 11[www.nature.com/naturecommunications](www.nature.com/naturecommunications)Additional information Supplementary information The online version contains supplementary material available at https://doi.org/10.1038/s41467-026-74500-3. Correspondence and requests for materials should be addressed to Kohei Shimokawa, Yasunori Kikuchi or Akihiro Okamoto. Peer review information Nature Communications thanks the anon- ymous reviewers for their contribution to the peer review of this work. A peer review file is available. Reprints and permissions information is available at http://www.nature.com/reprints Publisher’s note Springer Nature remains neutral with regard to jur- isdictional claims in published maps and institutional affiliations. Open Access This article is licensed under a Creative Commons Attribution-NonCommercial-NoDerivatives 4.0 International License, which permits any non-commercial use, sharing, distribution and reproduction in any medium or format, as long as you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons licence, and indicate if you modified the licensed material. Youdonot havepermissionunder this licence toshare adapted material derived from this article or parts of it. The images or other third party material in this article are included in the article’s Creative Commons licence, unless indicated otherwise in a credit line to the material. If material is not included in the article’s Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http:// creativecommons.org/licenses/by-nc-nd/4.0/. © The Author(s) 2026 Article https://doi.org/10.1038/s41467-026-74500-3 Nature Communications \|         (2026) 17:5400 12[https://doi.org/10.1038/s41467-026-74500-3](https://doi.org/10.1038/s41467-026-74500-3)[http://www.nature.com/reprints](http://www.nature.com/reprints)[http://creativecommons.org/licenses/by-nc-nd/4.0/](http://creativecommons.org/licenses/by-nc-nd/4.0/)[http://creativecommons.org/licenses/by-nc-nd/4.0/](http://creativecommons.org/licenses/by-nc-nd/4.0/)[www.nature.com/naturecommunications](www.nature.com/naturecommunications)- Electrode-free bioelectrochemical intercalation for scalable lithium recovery- Results- MR-1 drives electrode-free Li intercalation- Cell–material interface and electron transfer- EET controls Li intercalation- Scale-up potential of self-assembled agglomerates- Robust Li recovery from real seawater- Energetic basis and generality of bioelectrochemical intercalation- Techno-economic and life-cycle assessments- Discussion- Methods- Synthesis- Bacterial preparation- Shewanella oneidensis- Bioelectrochemical Li recovery- Characterisation- Techno-economic and life-cycle analyses- Statistics and reproducibility- Reporting summary- Data availability- References- Acknowledgements- Author contributions- Competing interests- Additional information