# Fileset

[20267Toda-ISIJInt.pdf](https://mdr.nims.go.jp/filesets/9563e6fb-f5f1-4eab-9cec-a923bf1f20e7/download)

## Creator

[Yoshiaki Toda](https://orcid.org/0000-0002-8343-2890), Nina Kobata, [Xianglan Li](https://orcid.org/0000-0003-0992-1722), [Masahiko Demura](https://orcid.org/0000-0002-7308-3041)

## Rights

[Creative Commons BY-NC-ND Attribution-NonCommercial-NoDerivs 4.0 International](https://creativecommons.org/licenses/by-nc-nd/4.0/)

## Other metadata

[Effect of Pressure on Steam/Supercritical Water Oxidation of 9Cr Steel and 18Cr Steel at 650°C](https://mdr.nims.go.jp/datasets/7c3e271c-7002-4722-a2a9-e180a8711670)

## Fulltext

ISIJ Int. 66(12): 1627-1637 (2026)  1627 \* Corresponding author: E-mail: TODA.Yoshiaki@nims.go.jp © 2026 The Iron and Steel Institute of Japan. This is an open access article under the terms of the Creative Commons  Attribution-NonCommercial-NoDerivs license (https://creativecommons.org/licenses/by-nc-nd/4.0/). ISIJ International, Vol. 66 (2026), No. 12, pp. 1627–1637 https://doi.org/10.2355/isijinternational.ISIJINT-2026-179 1\.  Introduction Understanding the steam oxidation behavior of heat- resistant materials is important for the safe long-term opera- tion of boilers and pressure vessels. Therefore, many studies  have been conducted on the oxidation behavior of heat- resistant metallic materials in high-temperature steam.1,2)  In addition, recent high-efficiency thermal power plants  generate supercritical water above 600°C and 25 MPa in  boilers to drive power generation turbines.3–6) Furthermore,  the use of supercritical water is also expected in light water  reactors,7,8) and in geothermal power generation systems,9,10)  which are effective for achieving carbon neutrality. There- fore, it is important to understand not only the oxidation of  heat-resistant metallic materials in high-temperature steam  but also their oxidation in supercritical water. Many studies have investigated the oxidation behavior  in supercritical water of 9Cr and 12Cr ferritic/martensitic  steels and 18Cr austenitic steel, which have been widely  used as boiler and pressure vessel materials in supercriti- cal thermal power plants and are candidate cladding and  Effect of Pressure on Steam/Supercritical Water Oxidation of 9Cr  Steel and 18Cr Steel at 650°C Yoshiaki TODA,1)\*  Nina KOBATA,1) Xianglan LI2)  and Masahiko DEMURA3)  1\)  Center for Basic Research on Materials, National Institute for Materials Science, 1-2-1 Sengen, Tsukuba, Ibaraki 305-0047,  Japan. 2)  Advanced Engineering and Service Division, National Institute for Materials Science, 1-2-1 Sengen, Tsukuba, Ibaraki 305- 0047, Japan. 3) Center for Basic Research on Materials, National Institute for Materials Science, 1-1 Namiki, Tsukuba, Ibaraki 305-0044, Japan. (Received June 24, 2026; Accepted September 7, 2026; Advance online published September 15,  2026; Published November 15, 2026) 9Cr ferritic/martensitic steel and 18Cr austenitic steel were exposed to steam (0.5 MPa), subcritical  water (10.2 MPa), and supercritical water (22.7 MPa) at 650°C for various durations. The pressure depen- dence of the oxidation rate constants of both steels was determined from the time dependence of  specimen weight gain and oxide scale thickness due to oxidation. The oxidation rate constants of both  steels decreased with increasing pressure. In steam, the oxidation rate constant of the 18Cr steel was  smaller than that of the 9Cr steel. The difference in the oxidation rate constants between the two steels  decreased with increasing pressure, and the oxidation rate constants became almost identical in super- critical water. The decrease in the oxidation rate constant with increasing pressure is considered to result  from the reduction in voids in the formed oxide scales, which restricts the transport of metal and oxygen  ions through the oxide scales. KEY WORDS:  heat-resistant steel; oxide scale; oxidation rate constant; oxidation reaction exponent; pres- sure; supercritical water. structural materials for supercritical water reactors. The  temperature dependence, dissolved oxygen dependence,  and alloying/additional element dependence of the oxidation  rate have been examined, and the structure and composi- tion of oxide scales formed in supercritical water have been  characterized.7,8,11–21) Recently, the supercritical water oxi- dation behavior of various heat-resistant metallic materials  has also been analyzed and predicted using computational  materials science.22–25) However, there have been very few  systematic studies on the pressure dependence of oxidation  behavior, such as comparisons between steam oxidation  at atmospheric pressure and supercritical water oxidation  under high pressure, or their relationship with subcritical  water oxidation at intermediate pressures. For 9Cr and 12Cr  ferritic/martensitic steels at 500–540°C, it has been reported  that the oxidation rate in supercritical water at 25 MPa is  higher than that in high-temperature steam at approximately  10 MPa.16,17,21) In contrast, there are also reports that the oxi- dation of 9Cr and 12Cr ferritic/martensitic steels becomes  slower with increasing pressure.18,26) In this study, to further investigate the effect of pressure  on the oxidation behavior of heat-resistant steels, 9Cr fer- ritic/martensitic steel and 18Cr austenitic steel were exposed [https://creativecommons.org/licenses/by-nc-nd/4.0/](https://creativecommons.org/licenses/by-nc-nd/4.0/)[https://orcid.org/0000-0002-8343-2890](https://orcid.org/0000-0002-8343-2890)[https://orcid.org/0000-0003-0992-1722](https://orcid.org/0000-0003-0992-1722)[https://orcid.org/0000-0002-7308-3041](https://orcid.org/0000-0002-7308-3041)ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ 1628 for various durations at 650°C, which is close to the operat- ing temperature of actual supercritical thermal power plants,  to steam (0.5 MPa), subcritical water (10.2 MPa), and super- critical water (22.7 MPa) under different pressures. The time  dependence of weight gain and oxide scale thickness due to  oxidation was then measured. Based on these results, the  pressure dependence of the oxidation rate constants of each  specimen was evaluated. Observation and identification of  the oxide scales were performed to investigate the effect of  pressure on the oxidation behavior of heat-resistant steels  at 650°C. 2\.  Experimental Procedure In this study, a 9Cr-1Mo-V-Nb (mass%) ferritic/martensitic  steel for boilers and pressure vessels (ASME SA-387/SA- 387M Grade 91) and an 18Cr-8Ni (mass%) austenitic stain- less steel (JIS G4304 SUS304) were investigated (hereafter  referred to as 9Cr steel and 18Cr steel, respectively). The  average compositions of the materials used are listed in  Table 1. Strip-shaped specimens with dimensions of 20 ×  10 ×  2 mm were cut from these commercial plates using electri- cal discharge machining. All surfaces of the specimens were  mechanically polished with wet abrasive paper up to #600  grit to obtain approximately the same surface roughness  for all specimens. The length, width, and thickness of each  specimen were then measured with a precision of 1 μm to  determine the total surface area. After cleaning and degreas- ing in an ultrasonic cleaner, each specimen was placed indi- vidually in an alumina crucible with a diameter of 26 mm  and a depth of 19 mm, and dried at 150°C for 6 h using a  drying oven. The specimens, including the crucibles, were  then weighed using an electronic balance with a precision of  0.1 mg. Empty crucibles without specimens were also dried  and weighed in order to measure the weight change of the  crucibles themselves during the oxidation tests. Figure 1 shows a schematic illustration of the steam/ supercritical water oxidation test apparatus. In the pure  water tank, the dissolved oxygen concentration in the pure  water was reduced to less than 15 ppb by argon bubbling,  and the electrical conductivity was reduced to less than  10 mS/m using ion-exchange resin. The crucibles contain- ing the specimens and the empty crucibles were placed in a  vertical cylindrical pressure vessel made of a nickel-based  alloy with a volume of 2.8 L. The pressure vessel was  heated using an electric furnace, and after the temperature  inside the pressure vessel exceeded 200°C, pure water  was supplied from the tank to the pressure vessel using a  high-pressure pump. The pure water passed through a heat  exchanger and a preheater from the tank, was gradually  heated, and was supplied from the lower side of the pres- sure vessel. Steam discharged from the top of the pressure  vessel was cooled through the heat exchanger and a cooler,  and then returned to the pure water tank. In Fig. 1, the pip- ing of the apparatus is shown in blue (low temperature),  purple (medium temperature), and red (high temperature)  according to the steam temperature in the pipes. When  the inside of the pressure vessel was heated to 650°C, the  pressure inside the vessel reached 0.5 MPa. Furthermore,  by closing the back-pressure valve while operating the  high-pressure pump, the pressure vessel was pressurized  and filled with subcritical water (10.2 MPa) or supercriti- cal water (22.7 MPa). The specimens and crucibles were  Fig. 1.  Schematic illustration of the steam/supercritical water oxidation test apparatus. The piping of the apparatus is  shown in blue (low temperature), purple (medium temperature), and red (high temperature) according to the  steam/supercritical water temperature in the pipes. Table 1.  Average compositions of the materials used (mass%). Fe C Si Mn Ni Cr Mo V Nb Cu N 9Cr steel Bal. 0.10 0.24 0.44 0.04 8.74 0.94 0.21 0.076 – 0.058 18Cr steel Bal. 0.043 0.45 0.90 8.09 18.36 0.15 – 0.018 0.24 0.053ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ1629 exposed to these environments for 0 h (in this case, only  heating/pressurization and cooling/depressurization were  performed), 20 h, 50 h, 72 h, and 195 h. After oxidation for  a given period, the temperature inside the pressure vessel  was decreased to 200°C and the pressure was reduced to  atmospheric pressure. The steam inside the pressure vessel  was then replaced with argon gas, and the vessel was cooled  to room temperature. Figure 2(a) shows the time dependence of the temperature  and pressure inside the pressure vessel during the oxidation  test at 650°C and 22.7 MPa for 50 h, indicated by the bold  and narrow lines, respectively. Figure 2(b) shows the same  changes in temperature and pressure inside the pressure  vessel on the phase diagram of water. The solid curve near  the center of Fig. 2(b) is the saturated vapor pressure curve,  with the gas phase on the right side and the liquid phase on  the left side. The region enclosed by the lines corresponding  to temperatures above the critical temperature of 374.15°C  and pressures above the critical pressure of 22.12 MPa in  the upper right part of Fig. 2(b) is the supercritical water  region. The heating/pressurization path is indicated by the  solid circles, whereas the cooling/depressurization path is  indicated by the open circles. After the oxidation tests, the crucibles containing the  specimens and the empty crucibles were removed from the  pressure vessel and weighed using an electronic balance  with a precision of 0.1 mg. The oxidation weight gain per  unit area was calculated by dividing the weight difference  before and after the test for each specimen including the  crucible by the total surface area. The weight change of the  crucibles was also taken into account in the weight change  of the specimens. The oxidized specimens were embedded in an epoxy- based room-temperature-curing resin and sectioned using  a low-load precision cutting machine. Cross sections of the  oxide scales formed on the specimen surfaces were observed  using secondary electron (SE) imaging with a scanning  electron microscope (SEM, S-4700, Hitachi, Ltd.). The  compositions of the oxide scales were analyzed using an  energy-dispersive X-ray spectrometer (EDX, XFlash5030,  Bruker) attached to the SEM, and the structures of them  were analyzed using a Raman spectrometer (LabRAM HR,  Horiba, Ltd.). 3\.  Experimental Results 3\.1.  Appearance of Oxidized Specimens Figure 3 shows photographs of the 9Cr steel and 18Cr  steel specimens kept in the crucibles after exposure to steam  (0.5 MPa), subcritical water (10.2 MPa), and supercritical  water (22.7 MPa) for 0 h (only heating/pressurization and  cooling/depressurization), 20 h, 50 h, 72 h, and 195 h. The  specimen dimensions were 20 mm in length and 10 mm in  width. The 9Cr steel specimens oxidized in steam (0.5 MPa)  remained silver-white, almost identical to the unoxidized  state, up to 72 h. Partial spallation of the oxide scale was  observed from 20 h, and large surface undulations were  observed on the specimen surfaces after 72 h and 195 h. The  9Cr steel specimens oxidized in subcritical water (10.2 MPa)  were brown from the initial stage of oxidation and became  nearly black after 20 h. Partial spallation of the oxide scale  occurred after 50 h, although the amount was smaller than  that in the steam (0.5 MPa)-oxidized specimens. Surface  undulations were observed on the specimen surface after  oxidation for 195 h. The 9Cr steel specimens oxidized in  supercritical water (22.7 MPa) exhibited a dark brown or  dark gray appearance from the initial stage of oxidation. No  spallation of the oxide scale was observed even after 195 h. The 18Cr steel specimens oxidized in steam (0.5 MPa)  changed in color from silver-white to gray and then to  brown. Partial spallation of the oxide scale was observed  from 20 h, and the amount appeared to be greater than that  in the steam-oxidized 9Cr steel specimens. The color change  of the 18Cr steel specimens oxidized in subcritical water  (10.2 MPa) was similar to that of the subcritical-water- oxidized 9Cr steel specimens, whereas spallation of the  surface scale was more pronounced than in the 9Cr steel.  The 18Cr steel specimens oxidized in supercritical water  (22.7 MPa) also exhibited the same color change as the 9Cr  steel, and no spallation of the oxide scale was observed. 3\.2.  Time Dependence of Oxidation Weight Gain Figure 4 shows the oxidation weight gain per unit area as  a function of oxidation time at 650°C in steam (0.5 MPa),  subcritical water (10.2 MPa), and supercritical water  (22.7 MPa) for (a) 9Cr steel and (b) 18Cr steel, indicated  by filled/open triangles, squares, and circles, respectively.  In the time-series data obtained from the same sample  under the same test condition, data points showing values  smaller than the surrounding trend are indicated by open  Fig. 2.  (a) Time dependence of the temperature and pressure  inside the pressure vessel during the oxidation test at  650°C and 22.7 MPa for 50 h, and (b) changes in tempera- ture and pressure inside the pressure vessel shown on the  phase diagram of water.ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ 1630 symbols. For these samples, the spalled oxide scale may  not have remained in the crucible, and the oxidation weight  gain may therefore not have been measured accurately.  Since these data are suspected to underestimate the weight  gain, only the data indicated by filled symbols were used  for the analysis of the time dependence described below.  The specimens also oxidized and gained weight during the  heating/pressurization process before the oxidation tests,  and cooling/depressurization process after the tests. There- fore, it should be noted that the oxidation weight gain was  not 0 μg/mm2 even when the oxidation time at the target  temperature and pressure was 0 h. At all pressures, the oxidation weight gain of the 9Cr steel  was larger than that of the 18Cr steel. Note that the scales of  the vertical axes are different between (a) 9Cr steel and (b)  18Cr steel. For both steels, the oxidation weight gain was  the largest in steam (0.5 MPa), followed by subcritical water  (10.2 MPa) and supercritical water (22.7 MPa), in which the  oxidation weight gain decreased in this order. The time, t dependence of the oxidation weight gain, Δw  is often described by the following equation.12,14–17,19–21,26) &#32; �  �w w k t n w��  �  �0 ............................ (1) Here, Δw0 is the oxidation weight gain at an oxidation  time of 0 h, n is the oxidation reaction exponent, and kw is  the oxidation rate constant determined from the oxidation  weight gain. By rearranging Eq. (1), &#32; n w w k twlog log log�  ���  �  �  �0 ................. (2) is obtained. Therefore, the slopes, n were determined by  linear regression of the double-logarithmic plots of the  experimental data for oxidation weight gain, (Δw−Δw0) and  time, t shown in Fig. 4, and the results are listed in Table 2.  Fig. 3.  Appearance photographs of the 9Cr steel and 18Cr steel specimens after exposure at 650°C to steam (0.5 MPa),  subcritical water (10.2 MPa), and supercritical water (22.7 MPa) for 0 h (only heating/pressurization and cool- ing/depressurization), 20 h, 50 h, 72 h, and 195 h. Table 2.  Oxidation reaction exponent, n determined from oxida- tion weight gain, and oxidation rate constant, kw deter- mined assuming n =  2. Sample P \[MPa\] n kw \[μg2mm − 4h −1\] (assume n =  2) 9Cr steel 0\.5 1.68 4 827.01 10\.2 2.33 124.84 22\.7 1.67 3.87 18Cr steel 0\.5 1.73 35.95 10\.2 2.19 19.03 22\.7 1.56 3.44 Fig. 4.  Oxidation weight gain per unit area as a function of oxida- tion time at 650°C in steam (0.5 MPa), subcritical water  (10.2 MPa), and supercritical water (22.7 MPa), and their  regression curves for (a) 9Cr steel and (b) 18Cr steel.ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ1631 Under the steel grades and pressure conditions investigated  in this study, n ranged from 1.5 to 2.3. The variation in the  n values is considered to result from measurement errors in  the oxidation weight gain due to oxide scale spallation and  other factors, as well as measurement errors in the oxidation  weight gain Δw0 at an oxidation time of 0 h. As shown in Fig. 4, at all pressures, the change in oxi- dation weight gain of both steels clearly decreased with  increasing oxidation time. This indicates that, at all pres- sures investigated in this study, the oxidation process was  rate-controlled by mass transport through the oxide scales.  Therefore, it is reasonable to consider that the steam and  supercritical water oxidation observed in this study followed  the parabolic rate law with n =  2. In addition, previous  studies have analyzed the oxidation weight gain of metallic  materials in supercritical water using the parabolic rate law  with n =  2, as in the case of oxidation in steam at atmo- spheric pressure.12,15,17,19,26) Table 2 also lists the oxidation  rate constant, kw obtained by linear regression assuming n =  2. The dashed curves in Fig. 4 represent the parabolic curves  of Eq. (1) drawn using the obtained kw with the assumption  of n =  2. It can be seen that the weight gain due to oxidation  can be described by Eq. (1). Figure 5 shows the pressure dependence of the oxidation  rate constants of the 9Cr steel and 18Cr steel, indicated by  the triangles and circles, respectively. The oxidation rate  constants of both the 9Cr steel and the 18Cr steel decreased  monotonically with increasing pressure. The degree of  decrease was greater for the 9Cr steel than for the 18Cr  steel. Notably, in supercritical water (22.7 MPa), the oxi- dation rate constants of the 9Cr steel and the 18Cr steel  converged to nearly the same value. Thus, oxidation was  significantly suppressed in supercritical water, and the dif- ference between the two alloys disappeared. 3\.3.  Cross-sectional Microstructures of Oxide Scales Figure 6 shows SEM secondary electron images of cross  sections of oxide scales formed on the 9Cr steel after expo- sure to steam (0.5 MPa), subcritical water (10.2 MPa), and  supercritical water (22.7 MPa) at 650°C for 20 h, 50 h, and  195 h, respectively. The SEM images of the oxide scales  formed in steam (0.5 MPa) are shown at a different magni- fication from those formed at the other pressures. In each  image, the boundary between the black and gray regions  in the upper part corresponds to the specimen surface, and  the light gray region in the lower part corresponds to the  Fig. 5.  Pressure dependence of the oxidation rate constants deter- mined from the oxidation weight gain of the 9Cr steel and  18Cr steel at 650°C. Fig. 6.  SEM secondary electron images of cross sections of oxide scales formed on the 9Cr steel after exposure to steam  (0.5 MPa), subcritical water (10.2 MPa), and supercritical water (22.7 MPa) at 650°C for 20 h, 50 h, and 195 h,  respectively. The outer layer, inner layer, and metallic substrate are indicated by white arrows, respectively, on  the left side of the center SEM image.ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ 1632 metallic substrate. The region between them, where dark  gray contrast and voids are observed, corresponds to the  oxide scale, in which outer and inner layers were observed.  In one of the SEM images in Fig. 6, the outer layer, inner  layer, and metallic substrate are indicated by white arrows,  on the left side of the image. The oxide scale thickness of the 9Cr steel increased with  oxidation time from approximately 300 μm to approxi- mately 900 μm in steam (0.5 MPa), and from approximately  100 μm to approximately 200 μm in subcritical water  (10.2 MPa). In supercritical water (22.7 MPa), no clear  growth of the oxide scale was observed, and the oxide scale  thickness remained approximately 100 μm at all exposure  times. Voids were observed in the oxide scales formed on  the 9Cr steel in steam (0.5 MPa), particularly in the middle  region along the thickness direction. After 20 h, the voids  became horizontally continuous, resembling cracks. After  50 h, the thickness of the void regions increased, while their  continuity disappeared. The size of the voids located above  the central region of the oxide scale exceeded 100 μm. After  195 h, the size of the voids decreased, although voids were  observed throughout the entire oxide scale. In contrast, the  oxide scales formed in subcritical water (10.2 MPa) and  supercritical water (22.7 MPa) clearly contained fewer and  smaller voids. Figure 7 shows the results of EDX compositional analy- sis of cross sections of oxide scales formed on the 9Cr steel  after exposure to (a) steam (0.5 MPa) and (b) supercritical  water (22.7 MPa) for 50 h. Secondary electron (SE) images  and elemental mappings of iron, chromium, molybdenum,  and oxygen are presented together. In the oxygen mappings,  the colored regions correspond to the oxide scale, with the  free surface on the upper side and the metallic substrate on  the lower side. Although the oxide scales appeared to have  nearly uniform contrast in the SE images, the elemental  mappings revealed that the oxide scales consisted of two  layers, namely an outer layer and an inner layer. The outer  layer contained no chromium and consisted of iron oxide  containing a lower concentration of molybdenum than the  base steel. The inner layer consisted of iron oxide containing  a higher concentration of chromium than the base steel and  nearly the same concentration of molybdenum as the base  steel. In the oxide scales formed in (a) steam (0.5 MPa)  and (b) supercritical water (22.7 MPa) shown in Fig. 7, the  elemental concentration were almost the same in both the  outer and inner layers. The voids observed in the oxide scale  formed in steam (0.5 MPa) were predominantly formed on  the outer-layer side along the boundary between the inner  and outer layers. Figure 7(c) shows the results of Raman spectroscopic  analysis of the inner layer of the oxide scale formed in  supercritical water (22.7 MPa). Analysis of two other loca- tions in the inner layer of the oxide scale also revealed  peaks at wavenumbers of 313–322 cm −1, 541–549 cm −1,  and 669–680 cm −1, which were identified as magnetite- type iron oxide.27,28) Similarly, peaks at wavenumbers of  297–319 cm −1, 542–546 cm −1, and 666–669 cm −1 were  obtained from the outer layer of the oxide scale, and were  also identified as magnetite-type iron oxide.27,28) Similar  Raman spectra were obtained from both the inner and  outer layers of the oxide scales formed in steam (0.5 MPa),  and these were likewise identified as magnetite-type iron  oxide. Combined with the elemental mapping results, it is  considered that the outer layer consisted of chromium-free  magnetite-type iron oxide, Fe3O4, whereas the inner layer  consisted of magnetite-type iron oxide, (Fe, Cr)3O4, in  which chromium partially substituted for iron. The types  and structures of the oxides formed on the 9Cr steel were  Fig. 7.  Secondary electron (SE) images and elemental mappings of cross sections of oxide scales formed on the 9Cr  steel after exposure to (a) steam (0.5 MPa) and (b) supercritical water (22.7 MPa) for 50 h, and (c) Raman spec- troscopic profile obtained from the oxide scale formed in supercritical water.ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ1633 the same as those observed in previous studies on steam  oxidation and supercritical water oxidation.7,8,11,13,16,17) Figure 8 shows SEM secondary electron images of cross  sections of oxide scales formed on the 18Cr steel after  exposure to steam (0.5 MPa), subcritical water (10.2 MPa),  and supercritical water (22.7 MPa) at 650°C for 20 h, 50 h,  and 195 h, respectively. The interpretation of the images is  the same as that for the 9Cr steel shown in Fig. 6. The time  dependence of the oxide scale thickness of the 18Cr steel  was smaller than that of the 9Cr steel. The oxide scale thick- ness increased from approximately 70 μm to approximately  100 μm in steam (0.5 MPa), and from approximately 50 μm  to approximately 80 μm in subcritical water (10.2 MPa) and  supercritical water (22.7 MPa). Under all conditions, the  oxide scales were divided into inner and outer layers. Voids were observed in the oxide scales formed on the  18Cr steel in steam (0.5 MPa), particularly in the outer  layer and between the inner and outer layers. These voids  increased in size with increasing exposure time. In subcriti- cal water (10.2 MPa), the voids in the oxide scale became  larger after 50 h, whereas in supercritical water (22.7 MPa),  they became larger after 20 h; however, the voids subse- quently became smaller again with increasing exposure  time. In addition, the number of voids decreased and their  size became smaller with increasing pressure. Figure 9 shows the results of EDX compositional analy- sis of cross sections of oxide scales formed on the 18Cr steel  after exposure to (a) steam (0.5 MPa) and (b) supercritical  water (22.7 MPa) for 50 h, and the interpretation of the fig- ure is the same as that for the 9Cr steel in Fig. 7. The outer  layer consisted of iron oxide composed of iron and oxygen,  whereas the inner layer consisted of iron oxide containing  a higher concentration of chromium than the base steel and  nearly the same concentration of nickel as the base steel.  The elemental concentrations were almost the same in the  oxide scales formed in both (a) steam (0.5 MPa) and (b)  supercritical water (22.7 MPa). In both cases, the voids were  distributed within the outer layer. The results of Raman spectroscopic analysis of the outer  and inner layers of the oxide scale formed in supercritical  water (22.7 MPa) are shown in Figs. 9(c) and 9(d), respec- tively. Including two additional locations other than those  shown in Fig. 9(c), peaks were obtained from the outer  layer at wavenumbers of 300–319 cm −1, 542–546 cm −1,  and 666–669 cm −1. Therefore, the outer layer was identi- fied as magnetite-type iron oxide.27,28) Including two addi- tional locations other than those shown in Fig. 9(d), peaks  were obtained from the inner layer at wavenumbers of  599 cm −1 and 680 cm −1, and the inner layer was therefore  identified as spinel-type iron oxide.29,30) Combined with the  elemental mapping results, it is considered that the outer  layer consisted of Fe3O4, whereas the inner layer consisted  of FeCr2O4 partially substituted by nickel. These oxides  formed on the 18Cr steel were consistent with those reported  in previous studies.7,20) 3\.4.  Pressure Dependence of Oxide Scale Thickness  Change Figure 10 shows the change in oxide scale thickness  with oxidation time in steam (0.5 MPa), subcritical water  (10.2 MPa), and supercritical water (22.7 MPa) for (a) 9Cr  steel and (b) 18Cr steel, indicated by filled/open triangles,  squares, and circles, respectively. Similar to the oxidation  weight gain plots in Fig. 4, the open symbols indicate data  Fig. 8.  SEM secondary electron images of cross sections of oxide scales formed on the 18Cr steel after exposure to  steam (0.5 MPa), subcritical water (10.2 MPa), and supercritical water (22.7 MPa) at 650°C for 20 h, 50 h, and  195 h, respectively. The outer layer, inner layer, and metallic substrate are indicated by white arrows, respec- tively, on the left side of the center SEM image.ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ 1634 suspected to be underestimated based on the surround- ing trend, and these data were excluded from the analysis  described below. Since oxide scales were also formed dur- ing the heating/pressurization process before the oxidation  tests, and cooling/depressurization process after the tests,  the oxide scale thickness was not 0 μm even when the oxi- dation time was 0 h. The oxide scale thickness of the 9Cr  steel was larger than that of the 18Cr steel at all pressures.  For both steels, the oxide scale thickness was the largest in  steam (0.5 MPa), followed by subcritical water (10.2 MPa)  and supercritical water (22.7 MPa), in which the thickness  decreased in this order. The time, t dependence of the oxide scale thickness,  x was also assumed to follow Eq. (3), similarly to Eq.  (1).12,15,17,19,26) &#32; x x k t n x��  �  �0 ............................... (3) Here, x0 is the oxide scale thickness at an oxidation time  of 0 h, and kx is the oxidation rate constant determined  from the oxide scale thickness. As described in Section  3.2, the slopes, n were determined by linear regression of  the double-logarithmic plots of the oxide scale thickness,  (x−x0) and time, t shown in Fig. 10, and the results are  listed in Table 3. In the case of the 18Cr steel in super- critical water (22.7 MPa), n =  1.24, which was a relatively  low value, whereas under the other steel grades and pres- sure conditions, n was approximately 2. Therefore, the kx  was calculated from the experimental data of (x −x0) and t  assuming n =  2, and the results are listed in Table 3. The  interpretation of the variation in the n values obtained from  the experimental data in Table 3 and the validity of assum- ing n =  2 are the same as those described in Section 3.2.  The dashed curves in Fig. 10 represent the parabolic curves  Fig. 9.  Secondary electron (SE) images and elemental mappings of cross sections of oxide scales formed on the 18Cr  steel after exposure to (a) steam (0.5 MPa) and (b) supercritical water (22.7 MPa) for 50 h, and Raman spectro- scopic profiles obtained from the (c) outer layer and (d) inner layer of the oxide scale formed in supercritical  water. Fig. 10.  Changes in oxide scale thickness with oxidation time at  650°C in steam (0.5 MPa), subcritical water (10.2 MPa),  and supercritical water (22.7 MPa), and their regression  curves for (a) 9Cr steel and (b) 18Cr steel. Table 3.  Oxidation reaction exponent, n determined from oxide  scale thickness, and oxidation rate constant, kx deter- mined assuming n =  2. Sample P \[MPa\] n kx \[μm2h −1\] (assume n =  2) 9Cr steel 0\.5 2.22 2 666.66 10\.2 1.96 62.15 22\.7 2.17 1.70 18Cr steel 0\.5 2.34 22.65 10\.2 2.08 11.55 22\.7 1.24 1.95ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ1635 of Eq. (3) drawn under the condition of n =  2 using the  obtained kx. The time dependence of the oxide scale thick- ness is well described by Eq. (3). Figure 11 shows the pressure dependence of the oxida- tion rate constants determined from the oxide scale thick- nesses of the 9Cr steel and 18Cr steel, indicated by the  triangles and circles, respectively. Results similar to the  pressure dependence of the oxidation rate constants deter- mined from the oxidation weight gain shown in Fig. 5 were  obtained. The oxidation rate constants of both the 9Cr steel  and the 18Cr steel decreased monotonically with increasing  pressure. The degree of decrease was greater for the 9Cr  steel than for the 18Cr steel. As in the case of the oxidation  weight gain, the oxidation rate constants of the 9Cr steel  and the 18Cr steel became almost identical in supercritical  water (22.7 MPa). 4\.  Discussion 4\.1.  Voids in Oxide Scales The pressure dependence of the oxidation rate constants  at 650°C for 9Cr ferritic heat-resistant steel and 18Cr  austenitic steel, which are used as heat-resistant steels for  boilers and pressure vessels, was evaluated from the weight  change of the specimens (Fig. 4) and the change in oxide  scale thickness (Fig. 10). As a result, the oxidation rate  constants of both steels decreased with increasing pressure  (Figs. 5 and 11). This suggests that, at 650°C, which is close  to the actual operating temperature of supercritical thermal  power plants, boilers and pressure vessels can be safely  operated using higher-pressure subcritical water or super- critical water at the same temperature if they are designed  based on the oxidation behavior of heat-resistant steels in  steam at atmospheric pressure. At both steam and supercritical water pressures, the  oxides formed on the 9Cr steel were of the same type  and structure, showing no pressure dependence (Fig. 7).  In addition, the types of oxides formed on the 18Cr steel  also showed no pressure dependence. In other words, the  decrease in the oxidation rate constants with increasing  pressure was not caused by differences in the oxide types. Several voids were observed in the oxide scales formed  on the 9Cr steel in steam (0.5 MPa). In particular, large  Fig. 11.  Pressure dependence of the oxidation rate constants  determined from the oxide scale thicknesses of the 9Cr  steel and 18Cr steel at 650°C. Fig. 12.  Pressure dependence of the oxide scale densities of the  9Cr steel and 18Cr steel at 650°C. voids were observed in the outer-layer Fe3O4, in which  chromium was not substituted. However, in the oxide scales  formed in subcritical water (10.2 MPa) and supercritical  water (22.7 MPa), the voids became smaller and less numer- ous (Figs. 6 and 7). In the 18Cr steel as well, the number of  voids in the oxide scales decreased with increasing pressure  (Figs. 8 and 9). These differences in the amount and size of  the voids are considered to be related to the decrease in the  oxidation rate. The apparent density, ρ of the oxide scale can be cal- culated by dividing the oxidation rate constant determined  from the oxidation weight gain, kw (Fig. 5) by the oxidation  rate constant determined from the oxide scale thickness, kx  (Fig. 11). Figure 12 shows the pressure dependence of the  oxide scale density of the 9Cr steel and 18Cr steel formed  under the three pressure conditions indicated by the triangles  and circles, respectively. The oxide scale densities formed  on the 9Cr steel in steam (0.5 MPa) and supercritical water  (22.7 MPa) were 1.35 mg/mm3 and 1.51 mg/mm3, respec- tively. In previous studies, the oxide scale densities of 9Cr  steel (NF616) and 12Cr steel (HCM12A) were evaluated as  1.58 mg/mm311) and 1.37 mg/mm3,13) respectively. There- fore, the oxide scale density values shown in Fig. 12 are  considered reasonable. In addition, the oxide scale densities  formed on the 18Cr steel in steam (0.5 MPa) and supercriti- cal water (22.7 MPa) were 1.26 mg/mm3 and 1.33 mg/mm3,  respectively. The oxide scale densities of both the 9Cr steel  and the 18Cr steel increased monotonically with increasing  pressure. This increase in oxide scale density corresponds to  a decrease in the volume of voids in the oxide scales. The  decrease in the time dependence of the oxidation weight  gain (Fig. 4) and oxide scale thickness (Fig. 10) of the 9Cr  steel and 18Cr steel with increasing pressure, resulting in a  monotonic decrease in the oxidation rate constants (Figs. 5  and 11), is considered to be closely related to the monotonic  decrease in the volume of voids in the oxide scales (Fig. 12). During steam (0.5 MPa) oxidation, steam gas is con- sidered to directly penetrate into macroscopic voids in the  oxide scales, allowing oxidation to proceed through mass  transport faster than bulk diffusion through the oxide scales.  With increasing pressure, the volume of voids in the oxide  scales decreases, which is expected to suppress the mass  transport due to direct penetration of steam gas and thereby  decrease the oxidation rate.ISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ 1636 In the 9Cr steel, magnetite-type iron oxides, Fe3O4 and  (Fe, Cr)3O4, were formed. In the 18Cr steel, magnetite-type  iron oxide was formed in the outer layer, whereas FeCr2O4  spinel-type complex oxide was formed in the inner layer.  Since the diffusion of elements and ions is slower in the  spinel-type complex oxide than in the magnetite-type iron  oxide, the former has a greater effect in suppressing oxida- tion. Therefore, in steam (0.5 MPa), the oxidation rate con- stant of the 18Cr steel was smaller than that of the 9Cr steel. As described above, with increasing pressure, the void  volume in the oxide scales, particularly in the magnetite- type iron oxide, decreased, thereby suppressing oxidation.  Moreover, as shown in Fig. 12, the decrease in the void  volume in the oxide scales was greater for the 9Cr steel  than for the 18Cr steel. Therefore, with increasing pressure,  the oxidation rate constant of the 9Cr steel decreased more  markedly than that of the 18Cr steel. Under supercritical  water (22.7 MPa) conditions, the effect of oxidation sup- pression caused by the reduced void volume in the oxide  scales is considered to have become comparable to the pro- tective effect of the spinel-type complex oxide, resulting in  similar oxidation rate constants for the 9Cr steel and 18Cr  steel. Reducing the volume of macroscopic defects in the  oxide scale may enable even an iron-dominant oxide to act  as a protective oxide scale. 4\.2.  Comparison with Previous Studies To the best of the authors’ knowledge, no previous  studies focusing on the pressure dependence of steam/ supercritical water oxidation of 9Cr ferritic/martensitic  steel or 18Cr austenitic steel have been reported. Previous  studies that investigated oxidation behavior under different  pressures within a single paper are summarized in Table  4. The table lists the test conditions that are considered  to affect the oxidation behavior, including chromium con- tent, temperature, pressure, oxidation time, and dissolved  oxygen concentration. The type of experimental apparatus  (batch-type or flow-type) is also included as one of the test  conditions. Some previous studies on supercritical water  oxidation employed batch-type experiments using sealed  autoclaves.21,26) However, it has been pointed out that even  under the same supercritical water conditions, the oxidation  environment differs from that in flow-type oxidation test  apparatuses, resulting in differences in oxidation behavior.2)  On the right side of Table 4, the effects of increasing pres- sure on oxidation are categorized as either “accelerated”,  “suppressed”, or “independent”. In this study, the time dependence of oxidation weight  gain and oxide scale thickness of the 9Cr ferritic/martensitic  steel at three different pressures at 650°C was investigated  using the same experimental apparatus. As a result, increas- ing the pressure of steam/supercritical water suppressed the  oxidation of the 9Cr steel. In addition, previous studies have  also reported that increasing the pressure of steam/supercrit- ical water suppresses oxidation at high temperatures above  600°C.26) No previous studies investigating the pressure  dependence of void morphology in oxide scales were found.  However, for ferritic/martensitic steels at high temperatures  above 600°C, the reduction in voids with increasing pres- sure may suppress oxidation. In contrast, at temperatures  below 600°C, both results showing that increasing the pres- sure of steam/supercritical water accelerates oxidation16,17,21)  and results showing that it suppresses oxidation18) have  been reported. No clear relationship between the pressure  dependence of oxidation and the test conditions could be  identified from Table 4. At temperatures below 600°C,  mechanisms other than the reduction in voids are likely to  affect oxidation. For the 18Cr austenitic steel, Table 4 indicates that  increasing the pressure of steam/supercritical water sup- presses oxidation over a wide temperature range. No previ- ous studies investigating the pressure dependence of oxide  scale morphology in 18Cr austenitic steel were found.  However, it is considered that the reduction in voids with  increasing pressure suppresses oxidation over a wide tem- perature range. 5\.  Conclusions 9Cr ferritic/martensitic heat-resistant steel and 18Cr aus- Table 4.  Previous studies investigating steam/supercritical water oxidation of 9Cr ferritic/martensitic steel and 18Cr  austenitic steel under different pressures. Alloy Cr content   (mass%) Temp. \[°C\] Pressure   \[MPa\] Oxidation   duration \[h\] Dissolved Oxygen   content \[ppb\] Experimental   device type Effect of increasing   pressure on oxide References T91 8.90 400 25 and 30 780 8 000 Flow Independent 18\) 500 Suppressed NF616 8.82 500 10.8 and 25 2 000 10 Flow Accelerated 16, 17) T91 8.91 540 9.9 and 25 120 40 Batch Accelerated 21) Grade 91 8.74 650 0.5 and 10.2 and 22.7 195 15 Flow Suppressed This work NF616 9.02 600 1 and 10 250 7 Batch Suppressed 26\) 700 350 Independent HCM12A 10.83 500 10.8 and 25 2 000 10 Flow Accelerated 16, 17) HCM12A 10.78 600 1 and 10 250 7 Batch Suppressed 26\) 700 350 Independent 316L 16.68 400 and 500 25 and 30 780 8 000 Flow Suppressed 18) SUS304 18.36 650 0.5 and 10.2 and 22.7 195 15 Flow Suppressed This workISIJ International, Vol. 66 (2026), No. 12 ©  2026  ISIJ1637 tenitic steel were exposed for various durations in a pressure  vessel to steam (0.5 MPa), subcritical water (10.2 MPa),  and supercritical water (22.7 MPa) at 650°C. The pressure  dependence of the oxidation rate constants of each mate- rial was determined from the time dependence of specimen  weight gain and oxide scale thickness due to oxidation.  The oxidation rate constants of both steels decreased with  increasing pressure. In steam, the oxidation rate constant of  the 18Cr steel was smaller than that of the 9Cr steel. The  difference between the two steels decreased with increasing  pressure, and the oxidation rate constants of the two steels  became almost identical in supercritical water. These results  suggest that, at 650°C, boilers and pressure vessels can be  safely operated using higher-pressure steam or supercritical  water at the same temperature if they are designed based  on the oxidation behavior of heat-resistant steels in steam  at atmospheric pressure. The decrease in the oxidation rate  constants with increasing pressure is considered to result  from the reduction in voids in the formed oxide scales,  which is expected to suppress the mass transport due to  direct penetration of steam gas. Statement for Conflict of Interest The authors declare no conflicts of interest regarding this  manuscript. Acknowledgments This study was supported by JSPS KAKENHI Grant  Number 25K08550 and the 35th ISIJ Research Promotion  Grant from the Iron and Steel Institute of Japan. REFERENCES 1\)  S. R. J. Saunders, M. Monteiro and F. Rizzo: Prog. Mater Sci., 53  (2008), 775. https://doi.org/10.1016/j.pmatsci.2007.11.001 2\)  I. G. Wright and R. B. Dooley: Int. Mater. Rev., 55 (2010), 129.  https://doi.org/10.1179/095066010X12646898728165 3\)  F. Masuyama: ISIJ Int., 41 (2001), 612. https://doi.org/10.2355/ isijinternational.41.612 4\)  T.-U. Kern, M. Staubli and B. Scarlin: ISIJ Int., 42 (2002), 1515.  https://doi.org/10.2355/isijinternational.42.1515 5\)  R. Viswanathan, J. F. Henry, J. Tanzosh, G. Stanko, J. Shingledecker,  B. Vitalis and R. Purgert: J. Mater. Eng. Perform., 14 (2005), 281.  https://doi.org/10.1361/10599490524039 6\)  F. Abe: Engineering, 1 (2015), 211. https://doi.org/10.15302/j- eng-2015031 7\)  G. S. Was, P. Ampornrat, G. Gupta, S. Teysseyre, E. A. West, T. R.  Allen, K. Sridharan, L. Tan, Y. Chen, X. Ren and C. Pister: J. Nucl.  Mater., 371 (2007), 176. https://doi.org/10.1016/j.jnucmat.2007.05.017 8\)  C. Sun, R. Hui, W. Qu and S. Yick: Corros. Sci., 51 (2009), 2508.  https://doi.org/10.1016/j.corsci.2009.07.007 9\)  M. Hermanská, A. Stefánsson and S. Scott: Geothermics, 78 (2019),  101. https://doi.org/10.1016/j.geothermics.2018.11.002 10\)  Y. Yamaya: Surveys in Geophysics, 47 (2026), 595. https://doi. org/10.1007/s10712-025-09907-6 11\)  Y. Chen, K. Sridharan, T. Allen and S. Ukai: J. Nucl. Mater., 359  (2006), 50. https://doi.org/10.1016/j.jnucmat.2006.07.021 12\)  Y. Chen, K. Sridharan and T. Allen: Corros. Sci., 48 (2006), 2843.  https://doi.org/10.1016/j.corsci.2005.08.021 13\)  L. Tan, M. T. Machut, K. Sridharan and T. R. Allen: J. Nucl. Mater.,  371 (2007), 161. https://doi.org/10.1016/j.jnucmat.2007.05.001 14\)  P. Ampornrat and G. S. Was: J. Nucl. Mater., 371 (2007), 1. https:// doi.org/10.1016/j.jnucmat.2007.05.023 15\)  L. Tan, X. Ren and T. R. Allen: Corros. Sci., 52 (2010), 1520. https:// doi.org/10.1016/j.corsci.2009.12.032 16\)  J. Bischoff and A. T. Motta: J. Nucl. Mater., 424 (2012), 261. https:// doi.org/10.1016/j.jnucmat.2012.03.009 17\)  J. Bischoff, A. T. Motta, C. Eichfeld, R. J. Comstock, G. Cao and T.  R. Allen: J. Nucl. Mater., 441 (2013), 604. https://doi.org/10.1016/j. jnucmat.2012.09.037 18\)  D. Gómez-Briceño, F. Blázquez and A. Sáez-Maderuelo: J. Supercrit.  Fluids, 78 (2013), 103. https://doi.org/10.1016/j.supflu.2013.03.014 19\)  N.-q. Zhang, Z.-l. Zhu, H. Xu, X.-p. Mao and J. Li: Corros. Sci., 103  (2016), 124. https://doi.org/10.1016/j.corsci.2015.10.017 20\)  Y. Behnamian, A. Mostafaei, A. Kohandehghan, B. Amirkhiz, R.  Zahiri, W. Zheng, D. Guzonas, M. Chmielus, W. Chen and J. Luo:  J. Supercrit. Fluids, 119 (2017), 245. https://doi.org/10.1016/j. supflu.2016.10.002 21\)  Y. Li, S. Wang, P. Sun, J. Yang, X. Tang, D. Xu, Y. Guo, J. Yang  and D. D. Macdonald: Corros. Sci., 135 (2018), 136. https://doi. org/10.1016/j.corsci.2018.02.036 22\)  T. Yang and P. Dou: J. Iron Steel Res. Int., 32 (2025), 2609. https:// doi.org/10.1007/s42243-025-01464-x 23\)  J. Zhou, L. Ren, Y. Lv, W. Lin, W. Jian, D. Zhang, X. Suo, D. Ruan  and Q. Zhang: J. Nucl. Mater., 605 (2025), 155566. https://doi. org/10.1016/j.jnucmat.2024.155566 24\)  F. Hou, S. Ding, Y. Wang, X. Kou and Y. Li: J. Supercrit. Fluids,  236 (2026), 107037. https://doi.org/10.1016/j.supflu.2026.107037 25\)  M. Wang, P. Yang, R. Li, B. Li, B. Ren, Y. Duan, M. Li and Y.  Wang: Appl. Surf. Sci., 749 (2026), 167989. https://doi.org/10.1016/j. apsusc.2026.167989 26\)  Y. Yi, Y. Watanabe, T. Kondo, H. Kimura and M. Sato: J. Press.  Vessel Technol., 123 (2001), 391. https://doi.org/10.1115/1.1373656 27\)  F. Froment, A. Tournié and P. Colomban: J. Raman Spectrosc., 39  (2008), 560. https://doi.org/10.1002/jrs.1858 28\)  P. Colomban, S. Cherifi and G. Despert: J. Raman Spectrosc., 39  (2008), 881. https://doi.org/10.1002/jrs.1927 29\)  K. F. McCarty and D. R. Boehme: J. Solid State Chem., 79 (1989),  19. https://doi.org/10.1016/0022-4596(89)90245-4 30\)  Y. Matsuda, S. Hinotani and K. Yamanaka: Tetsu-to-Hagané, 79  (1993), 48. https://doi.org/10.2355/tetsutohagane1955.79.1\_48[https://doi.org/10.1016/j.pmatsci.2007.11.001](https://doi.org/10.1016/j.pmatsci.2007.11.001)[https://doi.org/10.1179/095066010X12646898728165](https://doi.org/10.1179/095066010X12646898728165)[https://doi.org/10.2355/isijinternational.41.612](https://doi.org/10.2355/isijinternational.41.612)[https://doi.org/10.2355/isijinternational.41.612](https://doi.org/10.2355/isijinternational.41.612)[https://doi.org/10.2355/isijinternational.42.1515](https://doi.org/10.2355/isijinternational.42.1515)[https://doi.org/10.1361/10599490524039](https://doi.org/10.1361/10599490524039)[https://doi.org/10.15302/j-eng-2015031](https://doi.org/10.15302/j-eng-2015031)[https://doi.org/10.15302/j-eng-2015031](https://doi.org/10.15302/j-eng-2015031)[https://doi.org/10.1016/j.jnucmat.2007.05.017](https://doi.org/10.1016/j.jnucmat.2007.05.017)[https://doi.org/10.1016/j.corsci.2009.07.007](https://doi.org/10.1016/j.corsci.2009.07.007)[https://doi.org/10.1016/j.geothermics.2018.11.002](https://doi.org/10.1016/j.geothermics.2018.11.002)[https://doi.org/10.1007/s10712-025-09907-6](https://doi.org/10.1007/s10712-025-09907-6)[https://doi.org/10.1007/s10712-025-09907-6](https://doi.org/10.1007/s10712-025-09907-6)[https://doi.org/10.1016/j.jnucmat.2006.07.021](https://doi.org/10.1016/j.jnucmat.2006.07.021)[https://doi.org/10.1016/j.corsci.2005.08.021](https://doi.org/10.1016/j.corsci.2005.08.021)[https://doi.org/10.1016/j.jnucmat.2007.05.001](https://doi.org/10.1016/j.jnucmat.2007.05.001)[https://doi.org/10.1016/j.jnucmat.2007.05.023](https://doi.org/10.1016/j.jnucmat.2007.05.023)[https://doi.org/10.1016/j.jnucmat.2007.05.023](https://doi.org/10.1016/j.jnucmat.2007.05.023)[https://doi.org/10.1016/j.corsci.2009.12.032](https://doi.org/10.1016/j.corsci.2009.12.032)[https://doi.org/10.1016/j.corsci.2009.12.032](https://doi.org/10.1016/j.corsci.2009.12.032)[https://doi.org/10.1016/j.jnucmat.2012.03.009](https://doi.org/10.1016/j.jnucmat.2012.03.009)[https://doi.org/10.1016/j.jnucmat.2012.03.009](https://doi.org/10.1016/j.jnucmat.2012.03.009)[https://doi.org/10.1016/j.jnucmat.2012.09.037](https://doi.org/10.1016/j.jnucmat.2012.09.037)[https://doi.org/10.1016/j.jnucmat.2012.09.037](https://doi.org/10.1016/j.jnucmat.2012.09.037)[https://doi.org/10.1016/j.supflu.2013.03.014](https://doi.org/10.1016/j.supflu.2013.03.014)[https://doi.org/10.1016/j.corsci.2015.10.017](https://doi.org/10.1016/j.corsci.2015.10.017)[https://doi.org/10.1016/j.supflu.2016.10.002](https://doi.org/10.1016/j.supflu.2016.10.002)[https://doi.org/10.1016/j.supflu.2016.10.002](https://doi.org/10.1016/j.supflu.2016.10.002)[https://doi.org/10.1016/j.corsci.2018.02.036](https://doi.org/10.1016/j.corsci.2018.02.036)[https://doi.org/10.1016/j.corsci.2018.02.036](https://doi.org/10.1016/j.corsci.2018.02.036)[https://doi.org/10.1007/s42243-025-01464-x](https://doi.org/10.1007/s42243-025-01464-x)[https://doi.org/10.1007/s42243-025-01464-x](https://doi.org/10.1007/s42243-025-01464-x)[https://doi.org/10.1016/j.jnucmat.2024.155566](https://doi.org/10.1016/j.jnucmat.2024.155566)[https://doi.org/10.1016/j.jnucmat.2024.155566](https://doi.org/10.1016/j.jnucmat.2024.155566)[https://doi.org/10.1016/j.supflu.2026.107037](https://doi.org/10.1016/j.supflu.2026.107037)[https://doi.org/10.1016/j.apsusc.2026.167989](https://doi.org/10.1016/j.apsusc.2026.167989)[https://doi.org/10.1016/j.apsusc.2026.167989](https://doi.org/10.1016/j.apsusc.2026.167989)[https://doi.org/10.1115/1.1373656](https://doi.org/10.1115/1.1373656)[https://doi.org/10.1002/jrs.1858](https://doi.org/10.1002/jrs.1858)[https://doi.org/10.1002/jrs.1927](https://doi.org/10.1002/jrs.1927)[https://doi.org/10.1016/0022-4596(89)90245-4](<https://doi.org/10.1016/0022-4596(89)90245-4>)[https://doi.org/10.2355/tetsutohagane1955.79.1\_48](https://doi.org/10.2355/tetsutohagane1955.79.1_48)